Iron soldering (manual / robotic)
In iron soldering, a heated soldering tip transfers energy directly to the solder joint. It remains the most common method for single-point soldering — both when carried out by hand and automatically. Two factors determine the result: how quickly and reliably the flux wets the surface, and how aggressively the solder attacks the soldering tip. Almit develops solder wires that address both of these factors — with high-performance fluxes for short soldering times and with the patented S+M Line for significantly longer soldering tip lifetime.
Hand soldering or robot soldering?
Iron soldering remains the most common method for single-point soldering – both manual and automated.
Hand soldering
The operator handles the soldering iron and wire. The sensory abilities of humans are often underestimated in automation.
Characteristics
- The result depends on experience and the operator’s form on the day
- No automatic data recording for traceability
Robot soldering
An axis system or robot moves a soldering head with a heat source and solder dispensing unit. Solder wire is fed via a wire feeder.
Characteristics
- Fully automatic via computer-based control
- Pinpoint-accurate and process-reliable, repeatable as often as required
- Data is stored – traceability included
In iron soldering, it is crucial to press the soldering iron with a defined force against both the pin to be soldered and the printed circuit board. In doing so, tolerances of the machine, as well as those of the printed circuit board to be soldered, must be taken into account. It is also crucial that the solder makes exact contact with the soldering tip during pre-wetting and with the solder joint during the actual soldering process.
Almit’s bestsellers for iron soldering
Almit stocks these five products for manual and robotic iron soldering.
-
Dual boost for unique wetting
Dual-Boost series
Two complementary activators: the solder flows immediately into the plated-through hole, and no bridges form during drag soldering.
Find out more
-
Top sellers for good reason
GUMMIX Series
No detaching, no cracking: GUMMIX-21 Zeta produces just three spatters during iron soldering at 380 °C.
Find out more
-
Life insurance for soldering tips
S+M Line
The patented micro-alloy minimises iron erosion from the soldering tip, whilst the M-Line also minimises oxidation.
Find out more
-
Up to 5 times longer soldering tip lifetime
LFM-23 S
The silver-free SnCuNi alloy, eutectic at 228 °C and unaffected by the price of silver.
Find out more
-
Lead-free with excellent strength
SJM series
No cracking even after 2,000 thermal cycles; silver content selectable from 0.3 to 4 %.
Find out more
What matters in robot soldering
Ideally, care is taken during the development of assemblies to ensure that they are designed for robot soldering.
- Accessibility It must be possible to position the soldering tip and solder wire at the solder joint.
- Thermal mass connection Keep this as small as possible; thermal reliefs on the printed circuit board can improve solderability.
- Positioning The tolerance should not exceed approximately 0.1 mm. For larger solder joints, a greater tolerance is permissible; in some cases, a camera inspection can correct for this.
- Temperature Set as low as possible to extend the tip’s service life and avoid stressing the components.
- Heat source Soldering iron, laser, high-frequency, thermode, hot air or flame – the choice depends on quantity, cycle time, budget and component.
- The solder This determines the soldering time required for the solder to flow through. Better wetting shortens the soldering time and extends the tip’s service life.
At least 1.8 % flux
For iron soldering, a solder wire with at least 2.5 % flux content is used. SR-37 or DB-1 RMA are recommended. Almit has been developing solder wires for robot soldering for many years.
- Wire via wire feeder
- Paste via a dispenser
- Select solder suitable for the heat source
How a soldering tip is constructed
The soldering tip is a wear part – but its service life can be significantly extended by using the correct soldering temperature and selecting the right solder wire.
- Copper core
- Tellurium copper, oxidation-reduced, easy to machine. Responsible for the soldering tip’s thermal conductivity.
- Iron layer
- Electroplated. Responsible for the service life. Leaching rates: 40–50 soldering cycles per µm of iron.
- Chromium layer
- Electroplated. Non-wettable part of the soldering tip, limits the wetting zone.
- Wetting zone
- The chromium-free zone. Responsible for the solderability of the soldering tip.
- Lead-free pre-tinning
- Responsible for activation and wetting ability in the as-supplied condition.
Three wear mechanisms
The copper core is coated with a layer of iron to protect against corrosion caused by the flux and against migration caused by the solder alloy. Due to a tin content of over 95 % in the lead-free solder, the leaching of the iron layer presents a new problem for the soldering tip lifetime.
- Chemical reaction – Corrosion caused by the flux
- Metallic reaction – Leaching by the solder alloy
- Mechanical stress – caused by the customer-specific application
Once the iron layer has been used up, the soldering tip has reached the end of its service life – as indicated by pitting in the copper core. For fine, conical soldering tips, the maximum iron layer thickness is physically limited and is less than 150 µm.
Temperature determines service life
The corrosion and leaching rates – and thus the wear on the soldering tip – depend on the alloy and the temperature. Wear increases disproportionately.
| 360 °C | 385 °C | 410 °C | |
|---|---|---|---|
| SnCu alloy | 19,000 | 13,850 | 7,450 |
With a SnCu alloy, the service life in the temperature range between 360 °C and 410 °C is reduced on average by 230 solder joints per °C – at the upper end of the range, around 40 % of the initial service life remains.
Above 385 °C only if the solder joint requires it
350–385 °C is recommended. Above this, wear on the soldering tip increases dramatically; the flux burns too quickly and leaves flux residues on the soldering tip. However, solder joints with a large mass dissipate a great deal of heat and require more power. In such cases, a soldering temperature of up to 450 °C may be justified – outside the measured range and to the detriment of the soldering tip lifetime.
Avoiding oxidation
- A soldering tip oxidises in an oxygen atmosphere and forms an oxide layer.
- This layer usually cannot be penetrated by the flux and remains non-wettable.
- Non-wettable soldering tips have significantly poorer heat transfer.
- A tip wetted with solder prevents the supply of oxygen to the wetting surface.
Practical tips for the workplace
- Use the widest possible tip shape – a chisel shape rather than a conical one.
- Dry cleaning helps maintain the soldering tip’s wetting ability.
- The soldering tip before the soldering process, not afterwards.
- Do not leave dry, cleaned soldering tips in the holder when the tool is not in use.
How the solder protects the soldering tip
It was previously thought that there was no way to prevent soldering tip erosion anyway. The patented S-Line has proven that using the right alloy significantly minimises soldering tip erosion.
What applies to the S-Line and erosion applies all the more to the M-Line with regard to oxidation: it can not only reduce oxidation but prevent it almost entirely. Behind this lies a patented micro-alloy – with one or two secret ingredients that Almit keeps to itself.
By using high-quality, lead-free solder wire, the soldering tip lifetime is almost restored to that achieved with leaded solder.
Test conditions: Comparison of soldering tips after 20,000 soldering operations: LFM-48 S (S-Line) versus a standard lead-free solder.
Your benefits with LFM-48 M
- Micro-alloyed solder
- Soldering tip lifetime is drastically increased
- Prevents solder tip oxidation
- Best results at low temperatures, shorter soldering time
LFM-48 M is available with a composition of Sn-3.0Ag-0.5Cu-α-β at 217–221 °C and flux contents of 2.5 %, 3.5 % and 4.5 %; LFM-22 S is available with Sn-0.7Cu at 227 °C and 3.5 %. Further details can be found in the expert reports ‘How to achieve optimum results even with the lead-free process’.
100 % continuous flux core
Conventional solder wires often suffer from the problem that the flux core is interrupted by air pockets. This leads to a lower quality of the solder joint during use.
Almit solder wires feature a 100 % continuous flux core without any air pockets whatsoever – the soldering process is not interrupted. This is made possible by a globally unique and particularly complex production process, in which the solder wires are manufactured under very high pressure.
Even wires as small as 0.08 mm in diameter have a continuous flux core. Almit’s extremely thin solder wires are used particularly in electronics, medical technology, the automotive industry and aerospace, opening up new possibilities for miniaturization.
Almit sets itself considerably higher standards than the industry: the flux core is always free from inclusions – regardless of the wire’s thickness and alloy.
Almit solder wires for iron soldering
SRS-ZL, QB-1 and DB-1 RMA are designed for iron, induction and laser soldering and are specifically designed for automated soldering.
The latest high-performance fluxes
DB-1 RMA
The unique one: Thanks to the innovative dual boost system, featuring one fast-acting and one long-lasting activator, DB-1 RMA achieves a new dimension in wetting. The process time is significantly reduced. Also suitable for laser soldering.
QB-1
The Exceptionally Efficient One: With Quick-Boost technology, QB-1 reaches peak activation in a very short time. This enables very rapid initial wetting, leading to significantly higher efficiency.
SRS-ZL
The Exceptionally Fast One: the halogen-free solder wire with exceptionally fast wetting behaviour. This L0 flagship product impresses with the properties of an L1 wire.
DB-ZERO
High performance entirely free of halogens: dual boost activation combines L0 purity with low-spatter, reliable soldering performance. Currently the top recommendation for halogen-free processes.
Flux classes according to IPC J-STD-004. For DB-ZERO, only the short form L0 has been classified to date.
Common characteristics
- Specially designed for automated soldering
- 100 % continuous flux core
- Virtually no flux spatter
- RoHS-compliant
Specification of high-performance fluxes
| Flux | Alloy | Composition | Melting range | Flux content | Diameter (Ø mm) |
|---|---|---|---|---|---|
| DB-1 RMA | LFM-48 M | Sn-3.0Ag-0.5Cu-α-β | 217–221 °C | 3.5 % | 0.3 · 0.38 · 0.5 · 0.65 · 0.8 · 1.0 · 1.2 · 1.6 |
| DB-1 RMA | LFM-23 S | Sn-0.6Cu-0.05Ni-α-β | 228 °C | 3.5 % | 0.3 · 0.38 · 0.5 · 0.65 · 0.8 · 1.0 · 1.2 · 1.6 |
| DB-1 RMA | SJM-03 S | Sn-0.3Ag-0.7Cu-2.0Bi-α | 210–226 °C | 3.5 % | 0.3 · 0.38 · 0.5 · 0.65 · 0.8 · 1.0 · 1.2 · 1.6 |
| QB-1 | LFM-48 M | Sn-3.0Ag-0.5Cu-α-β | 217–221 °C | 3.5 % | 0.3 · 0.38 · 0.5 · 0.65 · 0.8 · 1.0 · 1.2 · 1.6 |
| QB-1 | LFM-23 S | Sn-0.6Cu-0.05Ni-α-β | 228 °C | 3.5 % | 0.3 · 0.38 · 0.5 · 0.65 · 0.8 · 1.0 · 1.2 · 1.6 |
| SRS-ZL | LFM-48 M | Sn-3.0Ag-0.5Cu-α-β | 217–221 °C | 3.5 % | 0.15 · 0.2 · 0.3 · 0.38 · 0.5 · 0.65 · 0.8 · 1.0 · 1.2 · 1.6 |
| SRS-ZL | LFM-23 S | Sn-0.6Cu-0.05Ni-α-β | 228 °C | 3.5 % | 0.3 · 0.38 · 0.5 · 0.65 · 0.8 · 1.0 · 1.2 · 1.6 |
| SRS-ZL | SJM-03 S | Sn-0.3Ag-0.7Cu-2.0Bi-α | 210–226 °C | 3.5 % | 0.3 · 0.38 · 0.5 · 0.65 · 0.8 · 1.0 · 1.2 · 1.6 |
The rest of the range
| Flux | Class | Positioning |
|---|---|---|
| SR-37 | M1 | The tried-and-tested M1 classic: fast, reliable wetting on almost all surfaces. |
| NHR-TH | L0 | Specially designed for THT applications: reliable solder penetration, 100 % halogen-free. |
| SRS-RMA-NC | L1 | Particularly effective on through-hole printed circuit boards – reliable solder penetration even on multilayer boards. |
| SR-LA SUPER | M1 | Low-spatter melting behaviour for a clean working environment, reliable M1 activation. Successor to SR-LA. |
| SR-HS | — | For drag soldering processes: maximum soldering speed with a stable, consistent process and minimal spattering characteristics. |
| SR-38 RMA | L1 | Resin-based RMA wire producing a clean solder joint with clear, non-corrosive residues. |
| KR-19 | M1 | The classic choice for surfaces that are difficult to wet – from aluminium to nickel-plated surfaces, for both lead-free and leaded processes. |
| KR-19 RMA | L1 | The more powerful variant in the KR-19 range: optimal results on aluminium, nickel and stainless steel surfaces. |
| KR-19 SH RMA | L1 | The all-rounder for leaded processes: reliable activation, clean and clear solder joints. |
| BT-19 | L1 | Residues with high surface resistance (SIR) – for applications with high SIR requirements. |
| NHR-1 | L0 | Halogen-free L0 wire for residue-critical hand-soldering applications. |
| SW-09 | H0 | Highly activated for extremely difficult soldering tasks, halogen-free. Note: Residues must be cleaned off after soldering. |
| KR-28 | M1 | For high-lead, high-temperature solders (Sn8Pb92, 280–305 °C) – joints subject to high thermal stress. |
| GTH-RMA | L1 | Specially designed for indium-based solder wires (SABI alloy LFM-96, 202–210 °C). |
Diameter, grades, alloys
- 0.1 – 2.7 mm 0.1 · 0.15 · 0.2 · 0.3 · 0.38 · 0.5 · 0.65 · 0.8 · 1.0 · 1.2 · 1.6 · 2.0 · 2.7 mm. Special versions down to 0.08 mm.
- 1.1 – 4.5 % Flux content depending on the system and application.
- L0 to H0 Classifications according to IPC J-STD-004.
- All alloys Lead-free, ranging from SAC305 through the low-silver SJM series to silver-free SnCu systems; leaded from Sn63 to Sn8.
All alloys, with their compositions and melting ranges, can be found in the alloy table. The complete range is shown in the overview of lead-free and leaded solder wires.
Iron soldering – a brief answer
What is the correct soldering temperature for lead-free iron soldering?
350–385 °C is recommended. Above this, wear on the soldering tip increases dramatically, the flux burns off too quickly and leaves residues on the soldering tip. However, large solder joints dissipate a lot of heat and require more power. In such cases, a soldering temperature of up to 450 °C may be justified – outside the measured range of 360 to 410 °C and to the detriment of the soldering tip lifetime.
To what extent does an excessively high temperature reduce the soldering tip lifetime?
With an SnCu alloy, the service life in the range between 360 °C and 410 °C decreases by an average of 230 solder joints per °C – at the upper end of the range, around 40 % of the initial service life remains.
Why does a soldering tip wear out in the first place?
The copper core is protected against corrosion and migration by a layer of iron. Wear occurs as a result of chemical reactions (corrosion), metallic reactions (leaching) and mechanical stress. Once the iron layer has been worn away, the maximum service life has been reached – as indicated by the formation of holes in the copper core.
Can the solder affect the soldering tip lifetime?
Yes, significantly. In a comparative test after 20,000 soldering operations, the micro-alloyed S-Line (LFM-48 S) reduced soldering tip erosion by up to 86 % compared with a standard lead-free solder.
How should the soldering tip be cleaned?
Before the soldering process, not afterwards. Dry cleaning helps to maintain the soldering tip’s wetting ability. Dry, cleaned soldering tips should not be left in the holder when the tool is not in use.
What flux content is required for robot soldering?
For iron soldering, a solder wire containing at least 2.5 % flux is used. SR-37 or DB-1 RMA are recommended.
Which solder wire is suitable for automated iron soldering?
SRS-ZL (ROL0), QB-1 (ROM1) and DB-1 RMA (ROL1) are specifically designed for automated soldering and are suitable for iron, induction and laser soldering – with a 100 % continuous flux core and virtually no flux spatter.
Are there any halogen-free solder wires that perform as well as an L1 wire?
Yes. SRS-ZL is classified as ROL0 and offers the properties of an L1 wire combined with particularly fast wetting behaviour.
Which solder wire works on aluminium and stainless steel?
KR-19 reliably wets even surfaces that are difficult to wet, including aluminium. KR-19 RMA is the more powerful variant and delivers optimal results on aluminium, nickel and stainless steel surfaces.
How thin can a solder wire with a continuous flux core be?
Up to 0.08 mm in diameter. This is made possible by a particularly complex production process in which the solder wires are manufactured under very high pressure.
What positioning accuracy is required for a soldering robot?
The positioning of the component should not exceed a tolerance of approximately 0.1 mm. For larger solder joints, higher tolerances are permissible.
Which solder wire is suitable for your process?
Surface finish, through-hole requirements, cycle time and soldering tip costs determine the choice – for both hand soldering and robotic soldering. Please speak to your Almit specialist advisor.