Soldering Glossary
Soldering terminology
This ‘Terminology of Soldering’ is primarily aimed at engineers and technicians working in the field of surface-mount technology (SMT) in electronics, and its aim is to provide a general explanation of the various phenomena that occur during soldering. My sincere thanks go to President Makoto Sawamura and his colleagues from the research department at Nihon Almit Co Ltd.
Abietic acid
The main component of the coniferous resin used as a soldering flux. C20H30O2, molecular weight 302, melting point 174–175 °C. Insoluble in water, but soluble in chloroform and alcohol. Inactive towards metals at room temperature, but reacts above its melting point with CuO, SnO and PbO to form the respective metal salts and water.
CuO + 2 C19H29COOH → Cu(C19H29COO)₂ + H₂O
The chemical reaction that occurs here is attributable to the carboxylic acid group in abietic acid and increases the strength of the solder joint.
The behaviour of a binary alloy consisting of metals A and B is described by a phase diagram. But how is such a diagram produced? It is derived from the cooling curves of the alloys, which initially exist as a melt. The figure shows the cooling curves of the three alloys X, Y (eutectic) and Z, each of which has a different composition. The points XA and ZB represent the points where the cooling curves of X and Z, respectively, intersect the liquidus line (A’E and B’E). These are the temperatures at which metals A and B, respectively, begin to crystallise, i.e. they form primary crystals. When, during the solidification process, one structure precipitates out of another, heat of solidification is released and, consequently, the slope of the cooling curve decreases at this point. This kink can be used to determine the onset of crystallisation.
Leaching
If an alloy in which two metals, A and B, are mixed together – such as a eutectic alloy – is heated, A and B begin to melt even below their respective melting points. Similarly, when molten solder comes into contact with another metal, that metal melts and forms an alloy with the solder, even if it has a higher melting point than the solder. For example, the melting point of copper is 1083 °C, but it melts at just 250 °C when it comes into contact with molten solder. A silver coating on a printed circuit board also dissolves in the solder and forms an alloy with it. This process is known as leaching. In metallurgy, however, the term ‘leaching’ often refers to the extraction of a specific substance from a solution containing several components.
Snap-off
The distance between the underside of the stencil and the surface of the printed circuit board when printing on surface-mount printed circuit boards (‘snap’ means to click into place). In screen printing, this distance is often 20–50 mm. By maintaining this distance precisely, the PCB and stencil only come into contact during printing at the exact moment when the squeegee passes over the stencil.
Additive manufacturing
In addition to the most common method – the etching of copper substrates – printed circuit boards can also be manufactured by electroplating or chemical deposition of a conductor. Etching is also referred to as a subtractive process, whilst coating is known as an additive process. The latter method allows for the creation of extremely fine and complex conductor tracks. A further advantage is the reduced amount of etchant consumed in the process. Chemical plating, in particular, is referred to as a ‘full additive process’. → Subtractive process
Activated synthetic resin flux
Fluxes originally developed for CFC cleaning. As the cleaning effectiveness of CFCs has been called into question and the relevant regulations have been tightened, the use of such fluxes is hardly increasing. Their advantages are: 1.) no whitish residues form after cleaning, unlike with rosin-based fluxes, 2.) high heat resistance, 3.) improved wetting. On the other hand, the disadvantage is that the waxy or liquid residues left after soldering rule out the no-clean processing that is possible with rosin fluxes.
AlCoR brazing process
A method for brazing aluminium developed by the US company AlCoR, in which an extremely dry atmosphere with a dew point between –35 °C and –45 °C is generated in the brazing furnace, making it possible to braze aluminium in air. This method has the advantage of minimising the use of flux, thereby making cleaning after brazing easier.
Abietic acid
The main component of the coniferous resin used as a soldering flux. C20H30O2, molecular weight 302, melting point 174–175 °C. Insoluble in water, but soluble in chloroform and alcohol. Inactive towards metals at room temperature, but reacts above its melting point with CuO, SnO and PbO to form the respective metal salts and water.
CuO + 2 C19H29COOH → Cu(C19H29COO)2 + H2O
The resulting chemical reaction is attributable to the carboxylic acid group in abietic acid and increases the strength of the solder joint.
Allotrope (allotropic)
Allotropes are defined as different forms of the same element that differ in their crystal lattice structure or bonding behaviour. In most cases, these forms transform into one another at a specific temperature. Tin, for example, occurs as α-tin (grey tin) with a cubic crystal lattice and as β-tin (white tin) with a tetragonal crystal lattice. The latter is metallic tin, which is also used in soldering and has a shiny surface, but transforms into α-tin at a storage temperature of -30 °C. Arsenic also has three different allotropes, which are grey, yellow and black in colour respectively. Grey arsenic is the common metallic form (hexagonal crystal system), whilst yellow arsenic is a cubic crystal. The latter reverts to grey arsenic simply by exposure to light. Iron occurs as α-Fe (ferrite) with a body-centred cubic lattice and as γ-Fe (austenite) with a face-centred cubic lattice. → Tin pest.
Amorphous alloy
When metals – as well as ceramics and other materials – are heated beyond their melting point, their atoms begin to move in a disorderly manner (Brownian motion). As soon as the material cools down, these atoms immediately reform a regular atomic lattice, much like children playing in the school playground who line up in a row at the teacher’s call.
Of course, the formation of the crystal lattice does not happen instantaneously. During the transition from the molten state to the solid state, the atoms of the metal or ceramic material require a certain finite amount of time to assume their ordered positions.
For metals, this time span is of the order of one hundred-thousandth or one-millionth of a second. The cooling rate is therefore 10⁵–10⁸ °C/sec. However, there are no precise research findings on this. If the material is quenched faster than this cooling rate, a transitional state results:
This transitional state is both polycrystalline, like an ordinary metal, and non-crystalline, and is therefore referred to as an amorphous alloy. As such rapid quenching is practically impossible to achieve, silicon or boron are used as interstitial elements to enable an amorphous state to be achieved even at a lower cooling rate. As the figure shows, amorphous alloys are produced by pouring the melt onto a rapidly rotating roller, resulting in extremely thin metal foils. The alloys produced in this way possess 1.) good mechanical properties, 2.) high corrosion resistance and 3.) high electrical resistance. Today, they are used, for example, in acoustic recording heads.
Anisotropic conducting film
An adhesive film approximately 20–30 µm thick, containing a filler consisting of conductive particles 3–15 µm thick. In their initial state, the particles are dispersed within the adhesive, so that the film as a whole behaves as an insulator. The adhesive film is applied between the conductor patterns to be joined and then pressed together whilst heat is applied. This joins the upper and lower conductor tracks and simultaneously creates a conductive connection. Thermosetting epoxy or acrylic resins are used as the adhesive. Processing takes place at a temperature of approximately 150 °C and a pressure of approximately 20–50 kg/cm². This method was originally developed in 1977 but had to be adapted to the ever-decreasing pitch distances on printed circuit boards. With this process, the pitch can be as narrow as 0.1 mm. Carbon fibre particles were initially used as fillers, but solder powder has become more common in recent times. Its particles deform under heat and pressure, thereby forming conductive bonds more easily. Metallised particles are also used. The process is now frequently used in plasma display assemblies.
Tarnish (tarnish layer)
A very thin oxide layer that forms on metals in storage. Strictly speaking, it would be more accurate to refer to this as amorphous material rather than oxides. Despite its thinness, the tarnish layer impairs solderability. In ultrasonic soldering, for example, failure to join may occur because the power is too low.
Antimony effect
It is well known that adding antimony (Sb) to a Sn-Pb alloy increases its mechanical strength. But up to what Sb content does this effect persist? In Sn-Pb solder alloys, the strength of the solder increases up to an antimony content of 6 % of the tin content, particularly in terms of resistance to creep deformation. In a solder alloy such as 60Sn-40Pb, this corresponds to 60 × 0.06, i.e. 3.5 % antimony content. This is known as the antimony effect.
Antithixotropy (anti-thixotropy)
This term is used in relation to solder paste and describes the phenomenon whereby the apparent viscosity increases as the flow rate rises. The reason for this is that rod- or plate-shaped particles in the solder paste assume a specific orientation as a result of movement, causing the fluid to gel or harden more quickly.
Equivalent (chemical equivalent)
A unit used, amongst other things, in the MIL standard for specifying the composition of fluxes. An equivalent is the quantity X, in grams, of any given element that reacts with 7.999 g of oxygen (equivalent to ½ mole of oxygen). This quantity X is defined as 1 equivalent (unit: val) of the element in question. For elements that do not react directly with oxygen, the equivalent can be determined indirectly via an intermediate reactant. The equivalent corresponds to the quotient of the atomic mass of the element and its valence.
Occupational exposure limit (permissible exposure limit)
The abbreviations AGW and PEL are commonly used.
PEL values for soldering
Metal vapour (as oxide)________PEL (mg/m³)
Cd_____________________________0.100
Be_____________________________0.002
Zn_____________________________5.000
Sb_____________________________0.500
As_____________________________0.010
Pb_____________________________0.050
In_____________________________0.100
Ag____________________________0.010
PEL values for soldering
This entry is based on the limit values applicable in the USA.
Such limit values exist, for example, for the concentration of metal vapour or metal dust in the air at the workplace. The measurement is the mass of metal vapour (mg) per cubic metre of air. OSHA specifies the above limit values for soldering. The amount of metal in the air is also referred to as airborne metal concentration.
Etch factor
When manufacturing printed circuit boards, there is a risk that the etching process will cause the openings in the conductor layer to become larger than the specified dimensions. This increase must be taken into account by factoring in an etching factor. For metal layer thicknesses of 0.125 mm or greater, the dimensions of rectangular apertures are reduced by 25 % of the layer thickness, and the radii of circular apertures are reduced by the same amount. Also known as the etching factor.
Auger effect
A phenomenon in which an excited atom, upon returning to its ground state, transfers its energy to one of its electrons and ejects it, rather than emitting a photon. This effect can be utilised to analyse the chemical composition of a material at a depth of several atomic lengths below the surface.
Auger electron spectroscopy
This technique involves investigating the momentum distribution, the momentum energy distribution and the exit angle distribution of electrons ejected via the Auger effect, in order to analyse a thin layer of a body’s surface. The momentum and energy distributions of the electrons can be measured using electric or magnetic fields, or a combination of both, and reveal a wealth of information, particularly about the surfaces of solids and adsorbed molecules. By increasing the sensitivity of the electron detector, it is also possible to carry out microanalysis of surfaces in metallurgy, organic chemistry and biochemistry.
Azeotrope (azeotropic)
One of the properties that a mixed cleaning fluid must possess for use in soldering. If such a fluid is distilled, the mixing ratio of the liquid and the vapour is identical at a specific temperature and composition, and the boiling point is either extremely high or extremely low. A mixture of ethanol and water has an extremely low boiling point (78.3 °C) when the ethanol content is 96 %. Azeotropic cleaning solutions are particularly useful for the vapour degreasing of solder joints. Despite their high price, the overall costs are low because they enable highly efficient cleaning.
Barrier
In semiconductor physics, this term is used to refer to potential thresholds; in soldering, however, it refers to a physical solder barrier that covers a blow hole, as in the sentence ‘The solder that encapsulates blow holes acts as an active barrier.’ (The solder encapsulates the blow hole, acting as an active barrier.)
Beilby Layer (Beilby’s layer)
When metals are rubbed together, the heat generated by friction causes metal oxides to form on their surfaces. G. Beilby initially believed that the thin surface layer that formed was a layer of amorphous metal. Electron microscopy later showed that this, too, is an oxide layer. It resembles the tarnish that forms through oxidation on fresh metal when it comes into contact with air. → Tarnish, amorphous alloy
Wettability
Metal can only be soldered if the solder can spread across the base material. This property is known as wetting and is quantitatively related to the contact angle → (the angle of the tangent of the solder to the base material). If → = 0, the wetting is 100 %. A wetting balance is used to measure wetting. → contact angle, meniscograph, wetting balance
Wetting
Wetting is a key element of the soldering process. It depends primarily on the properties of the solder and the base material, but naturally also on external factors such as contamination (grease on the surface to be soldered), a sufficient soldering temperature (depending on the size of the parts being soldered) or the amount of flux.
Wetting velocity (flux)
Spread rate of a flux when applied to a hot copper plate (e.g. 250 °C). According to the JIS standard, the area covered after 30 seconds is measured; in practice, however, it is important to understand exactly how the flux spreads. To ensure that a process step can be completed within a few seconds, flux X1 in the figure – which grows in area the fastest at the start – would be preferable to flux X2, which has the greater absolute spread. This fact is clearly demonstrated by measurements taken using the VEL-500 system developed by Nihon Almit and Shinku Riko.
Wetting balance (wettability tester, wetting balance tester, meniscographic tester)
As a rule, a so-called wetting balance is used to measure the wetting ability of a solder alloy, or the effect of the flux required for this purpose. In this process, a test specimen is suspended from one end of a balance and immersed in a solder bath below. The surface tension and buoyancy of the solder bath push the test specimen upwards. At the same time, an external force (dyn) is applied to the test specimen to hold it in position. The degree of wetting of the test specimen by the solder bath can be assessed on the basis of the force required to maintain its vertical position.
However, with the conventional method, the sensitivity of the force measurement is very limited, and there is a time lag relative to the actual movement of the test specimen. In today’s soldering processes, however, the efficiency of the flux and the associated time savings play a key role. Figure 2, for example, shows the wetting curves of two test specimens, each coated with the high-quality flux A and the low-quality flux B, as recorded by such a wetting balance. It is not possible to distinguish between the quality of the fluxes using this method. Manufacturers Nihon Almit and Shinku Riko have therefore jointly developed a new measurement method which directly determines the change in position of the test specimen using a differential transformer (see Fig. 3). This direct measurement is highly sensitive and also serves as a good indicator of the quality of the flux (see Fig. 4). The derivative of the movement curve (Fig. 5) provides direct information about the wetting rate at the start of the soldering process. The development of this measurement principle thus represented a major advance in research into soldering fluxes and solder alloys. → Meniscograph
Contact angle
The tangential angle between the metallic base material to be soldered and the molten solder. The smaller the contact angle, the greater the wetting ability of the solder with respect to the base material. Consequently, when soldering, it is not only the solder itself that is important, but also its interaction with the base material.
Bernoulli’s energy equation (Bernoulli’s theorem)
Daniel Bernoulli (1700–1782) was the first to investigate the mathematical description of fluid flow. His energy equation forms the basis for the design of modern wave soldering baths. For incompressible fluids, it is expressed as follows:
q²/2 + p/ρ + gZ = const.
Here, q is the flow velocity, p is the pressure, ρ is the density, g is the acceleration due to gravity and Z is the height above any horizontal plane. This states that, for an incompressible fluid, if the acceleration due to gravity g and the height Z (friction effect) are constant, the sum of q² and p remains constant, as the density does not change. The higher the flow velocity, the lower the pressure p. In wave soldering baths, particularly in hollow-wave soldering, this phenomenon can be put to good use. → Hollow-wave soldering
Binary composition diagram (binary composition representation)
An alloy consisting of two metals, A and B, is known as a binary alloy, the composition of which can be represented as a line. Let us consider an alloy consisting of X grams of metal A and Y grams of metal B (Fig. 1). If weights of X g and Y g are suspended from the two ends of the line AB, they are in equilibrium when the line is supported at the fulcrum S. The following then applies to the line segments m and n on either side of S:
mn = Y g / X g
As this ratio corresponds to the principle of a lever, it is also known as the lever ratio. The percentage proportions of A and B can be illustrated using a line, as shown in Fig. 2, where the length of the line corresponds to 100 %.
Binder (vehicle)
The word ‘vehicle’ literally refers to a means of transport, but also refers to excipients in medicines or binding oils in paints (e.g. varnish). In the context of paints, it refers to a substance that binds the colour pigments and forms a continuous layer, hence the German term ‘Bindemittel’ (binding agent). In solder paste, the flux is intended to fulfil this function. By analogy with the concept of a vehicle, the terms ‘carrier medium’ or ‘carrier substance’ are also used.
Bubble formation (void)
Not to be confused with blow holes, which form in molten solder. Voids between the layers of a printed circuit board in multi-layer SMT PCBs. If, during the manufacture of multi-layer PCBs, the pressing pressure rises significantly faster than the temperature, the synthetic resin flows too freely, the layer thickness becomes uncontrollable and thermal resistance is lost. If the temperature rises too slowly, this leads to bubbles forming between the individual layers of the printed circuit board. To prevent this, the application of heat and pressure must be carefully synchronised.
Borax
Na₂B₄O₇ · 10H₂O (borate). An important mineral for boron extraction. When brazing copper, if the copper is first immersed in a borate solution and then heated, it is easier to braze. This step in the process is known as boratisation. Its solubility in water is 4.7 g/100 g H₂O (20 °C). At water temperatures of 60 °C and above, Na₂B₄O₇ · 5H₂O is formed (specific gravity 1.81). When borate is heated to 350–400 °C, it becomes an anhydride. At 878 °C, it takes on a transparent, glass-like form. Owing to its ability to dissolve metal oxides, it is a commonly used flux for brazing.
Brown oxide treatment
Depending on the requirements, the inner layers of multilayer printed circuit boards should have either a glossy or a matt finish. Each of these surface finishes has specific properties. The former have 1.) good wetting, 2.) corrosion resistance and 3.) low thermal discolouration, whereas the latter 1.) react well with synthetic resins and 2.) are difficult to detach. The chemical treatment of the copper is therefore adapted to the respective requirements. Brown oxide treatment is one of the methods used to finish glossy copper surfaces and, in particular, enhances adhesion to synthetic resins. Its name refers to the brown colouration that the copper acquires as a result. The oxidising agents used for this purpose are listed in the table below. → Red ring formation, black oxide treatment
Oxidising agents for brown oxide treatment
Composition Treatment parameters Duration of resistance to red ring formation Peel strength
pH_______________________(Temperature)___(Time)
Copper acetate 30 g/l 45 °C______4 mins 30 mins 0.8–1.2 kg/cm² 4.9
Barium sulphide 24 g/l
Ammonium sulphide 24 g/l
Copper sulphate 24 g/l
Oxidising agents for brown oxide treatment
CAF migration
Generally referred to as CAF (conductive anodic filament). Conventional printed circuit boards are manufactured from glass-fibre-reinforced epoxy resin (glass-epoxy). However, as Figure 1 shows, adhesion problems can arise between the glass fibre and the plastic core, resulting in gaps into which moisture can penetrate during cleaning. During operation of the electronic device, migration then takes place along the fibres between the anode and cathode. Migration along the inner walls of via holes leads to the formation of spikes within the holes and can thus impair electrical conductivity. Figure 2 shows a schematic representation of a damaged via hole and a photograph of it. (Takano, Shibata, Arai: Circuit Technology [Journal of the Japanese Society for Circuit Technology], 5 (6), pp. 337–334, 1990)
Castellation Soldering
A soldering technique in which components without connecting wires, e.g. leadless chip carriers, are attached with solder not only to the underside but also to the side walls. The word ‘castellation’ derives from ‘castle’ and alludes to the resemblance of the solder fillet to a fortress wall. In contrast, a solder joint on the underside of the component is called a blind solder joint, because it cannot be seen from the outside. → see also IPC J-STD-001E 7.5.6
CCB process
CCB stands for Controlled Collapse Bonding. It is a process developed by L.F. Miller and others at IBM, in which the molten solder changes shape under the influence of flux due to its surface tension. In the diagram illustrating the process, it can be seen that the solder joints are in the correct position after soldering in the reflow oven. This corresponds to the self-alignment effect during soldering. → Self-alignment effect
Chelate complex (chelate compound)
A type of activator used in fluxes, including in solder pastes, in which a polydentate ligand forms a coordinate bond. As a ligand such as NH2(CH2)2NH2 or O(CO)2O, as shown below, effectively ‘grabs hold of’ the metal atom Co or Cr, such complexes are known as chelates, from the Greek Χηλ → (chele), meaning ‘crab claw’.
Such chelating agents (chelate agents) can be used as precipitating agents, such as dimethylglyoxime, oxine and acetylacetone, but also for the isolation and purification of metal salts, as solder flux additives, as cleaning agents, as stabilisers or as masking agents. When a multidentate ligand binds to a metal ion, the resulting complex is more stable than a complex with an ordinary ligand. This is known as the chelation effect.
Chemical charring
When soldering with rosin flux, if the temperature becomes too high or the soldering time too long, the flux loses its effectiveness, particularly as it burns and carbonises. The formation of carbon-containing combustion products usually prevents a flawless solder joint. This process is known as chemical charring. When organic compounds are burnt and carbonised, charcoal is produced. This is where the English term ‘charring’ comes from.
Chip-on-Glass (chip-on-glass board)
Also known by the abbreviation COG. Depending on the process, an ITO (indium tin oxide) electrode is applied to a glass substrate and the chip is soldered to it, or a conductive adhesive is used to mount the chip. The illustration shows an example of the latter method, the stud bumping process.
Clearance
In soldering, ‘clearance’ usually refers to the distance between a component’s pin and the wall of a drill hole in through-hole assembly (through-hole technology). It can also refer to the thickness of a brazing alloy in brazed joints. Just as the thickness of the adhesive layer influences the strength of an adhesive bond, excessive clearance can also reduce the quality of the soldered joint. The figure illustrates this relationship: if the distance is sufficiently small, the shear strength of the joint significantly exceeds that of the filler materials.
Vapour-phase soldering (VPS) is used when assembling heat-sensitive components onto printed circuit boards. The vapour of inert fluoride liquids is used as the heat transfer medium, primarily the product Fluorinert FC-70 from 3M, which has a boiling point of 215 °C. This method offers the following advantages: 1.) In the vapour phase, the temperature is uniform; whilst this does not allow for the selective heating of individual components, it prevents heat damage to the printed circuit board. 2.) Less overheating than with infrared reflow soldering allows for easier removal of flux residues. 3.) As the solder does not oxidise in the vapour phase, a less active flux than usual can be used. 4.) Thanks to the uniform heating, smaller chips can be mounted beneath larger components. Disadvantages of the process include the currently high cost of the inert liquid and the risk of contamination from flux. However, precautions are being taken to prevent the vapour from escaping, additional heat sources are being used, and other improvements are being made.
A soldering process developed by Western Electric (USA) in 1975, in which perfluorocarbon, fluoropolyether, perfluorotriamylamine and other chemicals are used as vapour-phase media. These liquids are characterised by a wide temperature range, thermal stability, chemical inertness, non-flammability, low vapour pressure, low surface tension and high density, and are marketed under names such as Fluorinert (3M) and Multifluor (Ausimont), amongst others. As the heat of condensation (latent heat) released during the transition from the vapour phase to the liquid phase is utilised for heating, heat transfer is faster than in convection reflow soldering.
Deactivating flux
Halogens are regarded as essential components of soldering fluxes. Even where chlorides cannot be used, bromides or fluorides are still employed. As the halogens are not completely consumed during soldering, they may be present in the flux residues. To remove them completely, it is possible to add certain olefin compounds to the flux, which bind the halogens (see figure). Because these substances neutralise the halogens contained in flux residues, they are referred to as deactivators. Data indicate that, with deactivating fluxes, the halogen content in the solids content drops from 1.0 % before soldering to just 0.04 % after soldering. (Onishi and Takemoto: Papers from the Soldering Working Group at the 11th Research Conference on Microjoining organised by the Japan Welding Society, pp. 39–42.)
Debye–Scherrer method
A rod-shaped packed crystal powder or a multicrystalline sample is placed on the central axis of a cylindrically rolled film. The sample is then irradiated with monochromatic X-rays, producing a diffraction pattern. The various diffraction planes produce circular diffraction patterns with a scattering angle equal to twice the Bragg angle Q. These diffraction rings are also known as Debye–Scherrer rings. As their angular distribution varies depending on the composition and structure of the sample, they can be used to determine the nature of the sample. This analysis is also known as Debye–Scherrer X-ray diffraction analysis. It is used to determine the crystal structure of solder alloys.
Dielectric constant
The dielectric constant, also known as the permittivity (symbol ε), is a measure of the electrical excitation of a dielectric (insulator) when a voltage is applied to it. Its value is material-specific and should be as low as possible for solder residues, as assemblies are nowadays frequently soldered using RMA flux and encased in plastic without being cleaned. It is defined as:
ε = D/E
D: Dielectric flux density (C/m²), E: Electric field strength (V/m).
The ratio of the permittivity ε of a material to the permittivity ε₀ of air, ε_s = ε / ε₀
is called relative or specific permittivity. For air, this is 1.
Differential thermal analyser
Also known as DTA, after its English initials. It measures the temperature difference between a reference substance and a sample whilst they are being heated simultaneously, in order to draw conclusions about the thermal properties of the sample. When substances undergo a phase change due to heating, or when thermal decomposition occurs, they absorb or emit heat in the process. If, therefore, the same amount of heat is applied to the reference substance and the sample within a specific time, the thermal behaviour of the sample can be analysed by measuring the temperature difference between the two substances. This instrument can be used not only to determine structural changes and the melting temperature of a solder alloy, but also, amongst other things, to analyse the reaction behaviour of different fluxes as the temperature rises. The DTA curve is also known as a thermogram. Naturally, the galvanometer deflects in different directions depending on whether the reaction is endothermic or exothermic.
Diffusion coefficient
In diffusion between solids, such as during soldering, an activation energy E is required for the atoms to change their position. If a is the particle spacing and k is the Boltzmann constant, then D = a²τ₀ exp→(Ek T) is obtained as the diffusion coefficient, which is known to be highly temperature-dependent. The quantity 1τ₀ here indicates the hopping frequency of the particles. For example, the diffusion coefficient of C in Fe is approximately 0.02–0.1 cm²/day at 1000 °C. → Fick’s laws of diffusion
Dilatancy
A term describing a specific behaviour of suspensions. For example, when shear forces act on a liquid containing spherical particles packed at a high density, the particles move away from one another before they begin to slip. This phenomenon can also be observed in densely packed solder paste. In relation to the total particle mass, this results in an increase in volume due to the shear forces. Osborne Reynolds gave this phenomenon the name ‘dilatancy’. (O. Reynolds, Philosophical Magazine, Vol. 20, 1885, p. 469). Furthermore, in dense suspensions, the flow resistance increases under the influence of shear forces. When walking across a damp sandy beach, the sand expands beneath one’s feet, so that it retains the water within it and then appears to have dried out on the surface. This, too, is an effect of dilatancy. ‘Dilatant’ originally means ‘expanding’ and refers to an increase in the spaces between molecules, causing a body’s shape to change and its volume to increase. In a broader sense, this refers to the increase in viscosity resulting from shear forces. Such a fluid exhibits ‘dilatant flow behaviour’ (dilatant movement).
Wire bonding
Connection between the connection pads of an integrated circuit and the terminals inside the chip package using wires (Au, Au-Si, Al, etc.). This is achieved using various processes, such as thermocompression bonding, ultrasonic bonding and thermosonic bonding, which combines the first two processes.
Plated-through holes
Also known as PTH (short for ‘plated through hole’). A drilled hole in an insulating base material, the inner wall of which has been coated with copper or a double layer of copper and solder to establish a conductive connection between the outer and inner circuits. Ideally, this is an electroplated coating approximately 25–35 µm thick. The plated-through hole also serves as a mounting point for through-hole assembly.
Electrode potential
Also referred to as the single electrode potential. The internal potential of the electrode relative to the surrounding electrolyte phase. The internal potential of the electrode phase is denoted by Ve, and that of the electrolyte phase by Vs. There is a potential difference Ve–Vs between them. If, for example, a foreign metal is present in an electrolyte, both have different internal potentials and an electrolytic reaction takes place between them, i.e. a current flows, known as galvanic current. As the individual potential cannot be measured directly, it is determined using a reference electrode (e.g. a hydrogen electrode), which, together with the electrode to be measured, forms a galvanic cell. By measuring the voltage between the two poles, the electrode potential can be calculated as an absolute value. The following table provides an overview of various electrode potentials.
Standard electrode potentials
Electrode reaction Eo (volts) Electrode reaction Eo (volts)
Li+ +e Li -3.05 V3+ +e V2+ -0.26
K+ +e K -2.93 Ni²⁺ +2e Ni -0.25
Ba²⁺ +2e Ba -2.91 Sn²⁺ +2e Sn -0.14
Ca²⁺ +2e Ca -2.87 Pb²⁺ +2 Pb -0.13
Na⁺ +e Na -2.71 Fe³⁺ +3e Fe -0.06
Mg²⁺ +2e Mg -2.36 2H+ +2e H2 0.00
Al³⁺ +3e Al -1.66 Sn⁴⁺ +2e Sn²⁺ 0.15
Mn²⁺ +2e Mn -1.18 Cu²⁺ +e Cu⁺ 0.16
Cr²⁺ +2e Cr -0.91 Cu²⁺ +2e Cu 0.34
Zn²⁺ +2e Zn -0.76 Cu⁺ +e Cu 0.52
Cr³⁺ +3e Cr -0.74 Fe³⁺ +e Fe²⁺ 0.77
Fe²⁺ +2e Fe -0.44 Ag⁺ +e Ag 0.80
Cr³⁺ +e Cr²⁺ -0.41 2Hg²⁺ +2e Hg₂²⁺ 0.91
Cd²⁺ +2e Cd -0.40 Br₂(aq) +2e 2Br⁻ 1.09
Ti³⁺ +e Ti²⁺ -0.37 Pt²⁺ +2e Pt 1.20
Co²⁺ +2e Co -0.28 Co³⁺ +e Co²⁺ 1.81
Standard electrode potentials
Electromigration (migration)
The direct current flowing during the operation of a device can cause an electrolytic reaction to take place on the surface of the flux residues at a solder joint on a printed circuit board, particularly in high-humidity conditions. As shown in Figure 1, water containing chloride and fluoride ions is then present between two connecting wires. This acts as an electrolyte and results in a slight current flowing between the two wires. For example, after soldering silver-coated wires without subsequent cleaning, some of the flux residues dissolve due to ambient humidity and form ions. At the anode, the reaction Ag → Ag⁺ + e then takes place; copper dissolves and migrates through the electrolyte to the cathode, where it loses its charge and precipitates as metallic copper. From there, the copper grows as a tree-like crystal structure (dendrite) until it forms a conductive connection between the terminals and causes a short circuit. This disrupts the function of the printed circuit board.
Direct currents generally lead easily to electromigration at silver electrodes; however, this can also occur with tin solders. Microscopic images A and B show the migration of tin, using the example of a glass-fibre-reinforced epoxy resin printed circuit board with comb-shaped tracks and a track spacing of 0.4 mm, which was first coated with flux, then soldered at 250 °C using the wave soldering process, and subsequently subjected to a direct current voltage of 100 V for 96 hours at 60 °C and 95 % relative humidity. Electromigration passes through three distinct stages (see Fig. 2): I – initial stage, II – actual migration, III – slowed migration.
It can be seen that, whilst migration decreases in stage III, it does not come to a complete halt. Electromigration can be prevented as follows:
Use of non-polar polystyrene or polyethylene as the base material instead of polar phenolic resins. 1.) Removal of flux residues, which absorb moisture, through thorough cleaning. 2.) Coating of the spaces between conductors with solder resist. However, pores in the resist, even if they are tiny, promote electromigration and should therefore be avoided. 3.) Use of flux-cored solder with a flux that does not form hygroscopic residues, e.g. NoClean flux of the RMA type.
Electrophoresis
A phenomenon in which colloidal particles dispersed in a sol move towards an electrode when a voltage is applied to it. In colloidal solutions of Au, Sg, S, sulphides, SiO₂, etc., the particles move in the opposite direction to the electric field, whereas aluminium hydroxide and iron hydroxide follow the field. If a brightening agent is added to the electrolyte solution during electroplating, it is deposited by electrophoresis onto the areas with a thicker layer of metal, whilst metal continues to be deposited in the deeper areas. If the brightener is then removed with a brush after coating, a metal layer of uniform thickness remains. By adding hard tungsten carbide powder (WC) to the electrolyte solution, a hardened metal layer containing tungsten carbide can be produced by means of electrophoresis. Migration at solder joints is sometimes confused with the phenomenon of electrophoresis. → Electromigration
Electropolishing (electrolytic polishing)
A method used in particular for the preparation of specimens for microscopy, in which, for example, a specimen of pure tin, a single-phase alloy or a binary Sn-Pb alloy is placed as an anode in a suitable etching solution and a current is passed between this and a suitable cathode. Depending on the voltage and current density, metal is gradually and uniformly detached from the surface, resulting in a surface that is well suited for microscopy. However, etching is most intense at the edges of the specimen. This method is only applicable to certain alloys, as it is difficult to process specimens with two or more phases at the same removal rate. This can lead to incomplete polishing, as is the case with mechanical methods. If the structure consists of one or more phases, it is impossible to achieve a completely uniform removal of material from the surface, even when using special electrolytes or adhering to specific conditions, and this may result in specimens that are either unpolished or excessively etched. When two different phases come into contact with one another in the electrolyte solution, a galvanic reaction is unlikely to occur between them, and this reduces the chances of achieving a result of a quality comparable to that of mechanical polishing. Specimens that have been mechanically polished or successfully electro-polished are subsequently electro-etched. In this process, the specimen is placed in the appropriate etching solution and treated with a stronger current than during polishing. If the aim is to highlight only a specific phase of the alloy, electropolishing is easier to control and adjust quantitatively than chemical etching. The former offers the advantage of being able to isolate crystal grains, grain boundaries, individual phases, multiple layers or specific metallic components from the surrounding matrix. Furthermore, unlike mechanical polishing, it leaves no cracks in the polished surface. If one wishes to examine large quantities of similar samples on a regular basis, electropolishing is generally more effective than manual polishing and etching. Suitable polishing solutions and conditions for Sn alloys are listed in the table below. Three of the electrolyte solutions are chlorine-based and highly explosive at high temperatures, which is why particular caution is required. As no two samples are ever exactly the same, the electrolysis conditions must be adjusted for each one.
Electropolishing solutions for tin-based alloys
Components Cathode Voltage (V) Current density (A/dm²) Time Temperature (°C)
Perchloric acid (194 ml)
Acetic anhydride (806 ml) Sn 25–40 9–15 8–10 mins <25
Perchloric acid
(ratio 1.60) Al 50–60 40 10–15 sec. <35
Perchloric acid (63 ml)
Acetic acid (300 ml)
Water (12 ml) Sn 20–30 9–15 10 mins 25
Fluoroboric acid (40 ml)
Sulphuric acid (2 ml)
Water (58 ml) Stainless steel 15–21 400–700 3–5 sec. 20–45
Electropolishing solutions for tin-based alloys
Energy-dispersive X-ray spectrometry (EDX) (X-ray micro-analyser)
A photospectrometric method in which the sample under investigation is bombarded with an electron beam approximately 1 µm in diameter, so that the characteristic X-rays emitted from the irradiated area can then be quantitatively analysed using an X-ray spectrometer to determine the composition of the sample. What makes this method unique is that a very small, spatially confined section of the material can be analysed non-destructively. Consequently, the method is particularly well suited to the analysis of localised phenomena, such as the segregation of alloys or the diffusion layer of a solder joint. One disadvantage, however, is that whilst quantitative analysis is possible, it relates only to a single point on the sample and therefore requires various corrections. The accuracy is consequently lower than with X-ray fluorescence analysis. Furthermore, elements with an atomic number lower than that of magnesium can hardly be detected. By scanning the sample with the electron beam and varying the brightness of a Braun tube in proportion to the characteristic X-ray spectrum at each point, a continuous two-dimensional analysis (scan) is possible.
Work softening
Normally, metal becomes harder when it is worked at low temperatures. This is known as work hardening. The hardening caused by working is due to an increase in the dislocation density. In contrast, tin solders lose strength the more they are worked. This is referred to as softening. The reason for this is the recrystallisation of the worked tin at room temperature. If the worked tin is left to stand at room temperature, it recrystallises and becomes softer, as in the case of annealing. Al-Fe alloys (up to 10 % Fe) also undergo softening through forming due to recrystallisation at room temperature. → Recrystallisation, dislocation
Dewetting
Dewetting may occur following wetting by the solder. Metallurgical reactions at the wetting interface cause its energy state to change continuously. As the molten solder cools, its wetting energy decreases, whilst the cohesive force increases. As a result, the molten solder retreats and solidifies into large polyhedral beads. Small quantities of the reaction products of tin and lead remain on the previously wetted surface, giving it a tin-plated appearance. When viewed under magnification, the dewetted area appears to have many spots that were not covered by solder. Often, foreign particles trapped on the surface or a layer of dirt are the cause of the dewetting.
Epitaxy (epitaxial crystal growth)
Epitaxy refers to the growth of a crystal on the surface of a second crystal of a different chemical composition, whereby the crystal growth follows a precisely defined orientation. Such growth can be induced by precipitation from a solution, electroplating, surface oxidation, chemical vapour deposition or vacuum evaporation.
This form of crystal growth occurs particularly in substances whose lattice structure and lattice constants are similar to those of the substrate metal. Since the forces emanating from the substrate’s atoms act, at most, over a distance of a few atoms, the atoms of the growing crystal, under the influence of these forces, initially occupy the vacancies with the lowest potential, from where the crystal continues to grow. In the case of tin-lead coating, it is possible to first thermally decompose the metallic substrate by reaction with a halogen flux and then to deposit a tin-lead layer on top of it by epitaxy.
Heating by far-infrared radiation (far-infrared radiation heating)
The long-wavelength end of the visible light spectrum lies at approximately 0.76–0.8 µm. Beyond this range, the term ‘far-infrared’ is used. This radiation corresponds to the rotational spectrum of molecules, whilst the spectrum of molecular vibrations falls within the near-infrared range. Radiation at these wavelengths excites the molecules of a substance, causing them to move thermally and raising its temperature. When assembling printed circuit boards, individual areas can be heated in a short space of time in this way. For this reason, far-infrared radiation is widely used in reflow soldering ovens. IR is generally used to denote infrared.
Ethanol vapour shielded bonding process
It appears that, whilst migration does decrease in Stage III, it does not come to a complete halt. Electromigration can be prevented as follows:
1.) Use of non-polar polystyrene or polyethylene as the base material instead of polar phenolic resins. 2.) Removing flux residues that absorb moisture through thorough cleaning. 3.) Coating the spaces between conductors with solder resist. However, pores in the resist, even if they are tiny, promote electromigration and should therefore be avoided. 4.) Use of flux-cored solder with a flux that does not form hygroscopic residues, e.g. NoClean flux of the RMA type.
Eutectic
If two metals, A and B, are mixed in a specific ratio to produce an alloy, the melting point of the alloy is, in some cases, lower than the melting points of the individual metals. The alloy with the lowest melting point is called a eutectic alloy. A eutectic consisting of two metals, A and B, is referred to as a binary eutectic; one consisting of A, B and C is a ternary eutectic. The notation is E eutectic cooling heating A+B.
The figure shows the phase diagram (also known as a phase chart) for an alloy of lead and tin, from which it can be seen that a eutectic is formed when the tin content is 63 % (by mass) and the lead content is correspondingly adjusted.
Whilst the melting point of lead is 327 °C and that of tin is 232 °C, the melting point of the eutectic alloy is 183 °C. Until 2006, this was the most widely used alloy for solders. Within this eutectic alloy, lead and tin are merely very finely mixed together, without, however, reacting chemically. Eutectic alloys are therefore mechanical mixtures. The eutectic is the alloy with the lowest potential energy. It should be noted that at the eutectic temperature, Sn and Pb crystallise simultaneously from the melt; however, this does not happen instantaneously but takes some time. In zones a, at the ends of the phase diagram, Sn forms a solid solution in Pb, and vice versa.
Solids content
The volatile components of the flux evaporate during soldering, whilst the solids content remains as a residue. In conventional fluxes, these consist of rosin and the non-volatile components of the activators and surfactants. As rosin-based fluxes were previously the most common, the solids content was usually around 30 %. Nowadays, water-cleanable or no-clean fluxes are generally used, which is why fluxes with a solids content of less than 5 % – that is, low-rosin fluxes – are in demand.
Solid solution
A Pb-Sn solder alloy is eutectic. As mechanical mixing takes place in eutectic alloys, tin and lead can be clearly distinguished in a microscopic image. In some cases, however, two metals, A and B, mix so thoroughly that their respective structures disappear and a new, shared structure emerges. These are known as solid solutions. If, for example, alcohol is dissolved in water – that is, mixed completely homogeneously within it – the two substances are indistinguishable. It is impossible to remove some of the water from a whisky that has been diluted too much with water – you have to top it up with more whisky. An example of solid solutions of metals is nickel-copper alloys (constantan). In general, substances with the same lattice structure form solid solutions more readily. In Sn–Pb alloys, at the eutectic temperature, tin dissolves in lead with a mass fraction of 25 %. If the mixture is cooled and then reheated, tin is precipitated or redissolved each time. To determine the properties of a solder alloy, it is therefore necessary to allow the sample to stand for several hours or days.
This tendency to form solid solutions is also the reason why two metals with the same lattice type exhibit severe abrasion when rubbed against one another.
Flame resistance
When it comes to printed circuit boards, the terms ‘anti-combustion’ or ‘combustion resistance’ are not used; instead, the term ‘flame resistance’ is employed. This is because, for testing purposes, a flame is held against the printed circuit board until it ignites, and the time taken for the flame to go out is then measured. This property is important for assessing in advance the fire risk posed by the board catching fire due to overheating of the components mounted on it during use. This is also counteracted by adding flame-retardant halogen compounds to the base material. In the flame resistance test, a distinction is made between horizontal and vertical ignition, depending on how the circuit board is positioned. These tests are specified in JIS standard K6911, 5-24.
Fick’s law of diffusion
When soldering with a Sn-Pb solder on a copper plate, the intermetallic compound δ (Cu₄Sn) is formed between the copper and tin by diffusion. Fick’s law of diffusion is used to analyse this diffusion quantitatively. For the amount J of the solute (Cu) that diffuses into the melt (solder) per unit of time through a cross-sectional area perpendicular to the direction of diffusion, the following applies: J = –D grad C. Here, grad (gradient) is the concentration gradient (C) at this point and D is a proportionality constant (diffusion coefficient).
Flexible printed circuit board (FPCB)
A film made of polyester, polyimide or glass-fibre-reinforced plastic (e.g. glass-epoxy), onto which a copper foil circuit pattern has been formed. Before use, it is coated with an insulating film or a liquid protective varnish. Due to their relatively low cost, polyester films are frequently used as the base material; however, in recent times, the more expensive but more heat-resistant polyimide has also come into use in many applications. Flexible printed circuits can be used to connect rigid printed circuit boards or for movable designs in confined spaces. The copper foil is either electroplated or rolled onto the substrate. The base material and copper foil have thicknesses of 25–125 µm and 35–70 µm respectively.
Yield point (paste yield point)
The term is applied in particular to solder paste and differs from the stress-strain curve for metals. As the diagram shows, the yield point lies at the shoulder of the flow curve for solder paste, i.e. the curve of shear stress as a function of shear rate (γ). More reliable results are obtained when working at a low shear rate of approx. 50 mm/sec. It should be noted that a high yield point is not always related to the viscosity of the paste. In other words: as in the case of honey, a substance can have a high yield point and, at the same time, a high viscosity, but the opposite can also occur.
Flow behaviour (break-off)
Unlike beer, which some people would like to see flowing continuously, solder requires good dispensability – in English, this is referred to as a good ‘break-off’. Particularly in surface-mount assembly, the solder should break off cleanly and form neat solder cones (dots). Dispensing capability also plays a major role with solder paste. (Jennie S. Hwang: ‘Solder Paste in Electronics Packaging’, p. 340. Van Nostrand, Reinhold (ed.), Nihon Almit publication).
Flux
Flux
In soldering, flux and solder have always formed an inseparable unit. Solder paste, for example, consists of powdered solder mixed with a flux, whilst cored solder contains a flux core. Flux is composed of the following components:
Activator: A substance that serves to remove oxides from the metal to be soldered whilst simultaneously preventing oxidation during the soldering process. For a successful soldering process, the flux should melt first, allowing the solder to flow over it.
Binder: When water-white (WW) rosin is used as a binder, it also acts as an activator. In general, a binder serves a) as a carrier substance for heat and reaction products, b) to reduce the surface tension of the solder in order to promote its spread, and c) to protect the metal from re-oxidation at soldering temperature.
Solvents: primarily used as thinners for applying flux.
Solubilising agents: These prevent the binder from hardening before cleaning and enhance the cleaning effect. They also promote foam formation in foam flux systems during wave soldering and are used as co-solvents when the flux does not dissolve in the solvent. Esters, ethers and ether-alkanols, amongst others, are commonly used for the latter purpose.
Flux for soldering aluminium
Soldering aluminium is a very labour-intensive process. Based on current knowledge, the following fluxes are recommended (unit: ounce, oz)
Cadmium fluoride bromide
5 oz
fluorobromic acid 5
diethanolamine 20
diethanol diamine 4
diethanol triamine 10
potassium chloride
45 oz
sodium chloride 30
potassium fluoride 7
sodium pyrophosphate 3
triethanolamine
25 oz
fluorobromic acid 3
cadmium fluoride hydrochloride 2
stannous chloride
44 oz
ammonium chloride 5
sodium fluoride 1
zinc chloride
44 oz
ammonium chloride 5
Sodium fluoride 1
In addition, the following flux is available in paste form: (unit: ounce, oz)
Stannous chloride 83 oz
Zinc hydrazine dichloride
(deliquescent and water-soluble) 7
hydrogen bromide-hydrazine 10
water 10
Flux residues
Products of flux decomposition that remain on the solder joint after soldering. As they usually contain corrosive substances, their presence can compromise the long-term reliability of the solder joint; furthermore, in a hygroscopic environment, the residues can absorb moisture, leading to the formation of conductive bridges between the conductor tracks and resulting in the migration of copper and tin. For this reason, fluxes are required whose residues do not necessitate the use of CFC-containing cleaners, but can simply be removed with water. Such fluxes are referred to as water-soluble fluxes, although strictly speaking the term ‘flux that forms water-soluble residues’ would be more accurate. As residues make testing with nail-bed testers more difficult, they should be removed as far as possible. With RMA-type fluxes, on the other hand, cleaning is not necessary. If residues are not removed, however, their surface insulation resistance (SIR) must be tested at temperatures up to approximately 100 °C in a humid atmosphere, as even substances that insulate at room temperature can lose their insulating properties when the solder joint heats up.
Galvanic current
Named after its discoverer, the Italian physiologist L. Galvani (1737–1798). There are several accounts of this discovery. According to one version, Galvani became aware of the generation of an electric current due to a potential difference when the legs of a frog he was dissecting – which he had secured with clips made of different metals – suddenly twitched. Another account states that Galvani was dissecting the frog near an electric generator and that its legs twitched as a result of the electrical discharges.
A galvanic current is defined as an electric current flowing between electrodes made of different metals that are immersed in an electrolyte solution. If several different metals are placed in a row in the solution, the current flows through all these metal parts. In a very humid atmosphere, a tiny current can arise even without an electrolyte solution, and a galvanic cell is formed.
This phenomenon is also the reason why solder joints on equipment used outdoors are prone to faults. Even in stainless steel kitchen sinks, a potential difference can arise at the weld seams, leading to galvanic corrosion, even if the welding wire is made of the same material, because the structure of the steel sheet and the weld joint changes. Similarly, in solder joints using aluminium solders (Al-Zn-based), tiny currents occur at the interfaces between the different metals, triggering corrosion. To prevent this type of corrosion, the joint must be coated with a protective layer of plastic to ensure it does not come into contact with water.
Gas atomisation
Metal powder can be produced using both water atomisation and gas atomisation. The former method produces metal particles of irregular shape, which are suitable for compression moulding, whereas the latter generally results in round particles that possess the flow properties required for printing and can therefore be used, for example, in solder paste. The illustration shows the gas atomisation process.
Composition triangle for ternary alloys (ternary composite representation)
The composition of a ternary alloy consisting of the three metals A, B and C can be represented using an equilateral triangle. It is defined by a specific point X within the triangle. If a line parallel to each side is drawn through X, the respective proportion can be determined from the points of intersection on the sides. In this way, it is possible, for example, to easily determine the change in structure of a Pb-Sn alloy upon the addition of Sb.
Odour threshold (or concentration)
Rosin (coniferous resin), the main component of flux, gives off an odour when dissolved. The quantitative concentration of an odorous substance in the air is referred to as the odour concentration. If an odorous gas, when diluted 1,000-fold with ambient air, is no longer detectable by humans, then this substance has ‘an odour threshold of 1,000’. The greater the degree of dilution required, the stronger the odour of the substance in question. The dilution air used in this process is fed into an activated carbon tank by a special odourless pump to eliminate any traces of odorous substances. The assessment of whether or not an odour is present is carried out by a group of six or nine test subjects, usually women aged around 20.
Gibbs energy, Gibbs free energy, free enthalpy (Gibbs’ free energy)
Also known as thermodynamic potential or free energy at constant pressure. Gibbs free energy is defined as follows:
G = F + pV
Where p is the pressure, V is the volume and F is the Helmholtz free energy, for which F = U – TS.
Here, U is the internal energy, T is the absolute temperature and S is the entropy. → Surface tension
Lattice
Metals are polycrystals consisting of many crystal lattices. These lattices – arrangements of atoms – form, in a sense, the basic structure of a metal or an alloy. The atoms are arranged in specific, uniform patterns. Iron (Fe), for example, forms cubes at room temperature (see figure), with one atom at each corner and one at the centre. Iron therefore has a body-centred cubic lattice (bcc). Iron with this lattice structure is referred to as α-iron or ferrite. As the temperature rises, it adopts a face-centred cubic lattice structure and is then called austenite. Why iron exhibits a bcc structure at room temperature remains unclear according to the current state of scientific knowledge. → Lattice defects
Lattice defect
Materials consist of groups of a particular type of atom, the arrangement of which is known as a lattice. Based on a perfect lattice structure, the strength of a material can be calculated from the attractive and repulsive forces acting between its atoms. However, the actual strength of a material is considerably lower than this calculated value, as the atomic lattice contains vacancies and dislocations. Material failure is therefore often attributable to these defects.
Solder glass
Low-melting-point glass solders used to join glass-ceramics and metals. There are both non-crystalline glass solders and those that crystallise after joining. The term ‘soldering glasses’ is also used. Common chemical compositions of glass solders include B₂O₃-ZnO-SiO₂ and B₂O₃-PbO-SiO₂. → Soldering glass
When soldering components, particularly leadless chips, it can happen that, after one side has already been soldered in place, the other side lifts up, causing the component to stand at an angle on the printed circuit board. The chip then resembles a gravestone, which is why this fault is known by that name.
This phenomenon occurs when there is an uneven temperature distribution on the printed circuit board, the solder paste has been applied unevenly to the pad areas, the surface of the solder powder has oxidised due to preheating, or the solvent has partially evaporated, resulting in uneven soldering.
In this case, the solder on one pad of a pair of pads melts faster than on the other and, due to its surface tension, pulls the end of the chip downwards, causing it to stand upright (see fig.). As this phenomenon is reminiscent of New York’s closely packed rows of high-rise buildings, the name ‘Manhattan effect’ was coined. On the other hand, the chips standing at an angle resemble gravestones, which is why the name ‘tombstone effect’ is also commonly used. This usually occurs when the solder wets the pad on only one side.
Tombstone effect (tombstoning)
When soldering components, particularly leadless chips, it can happen that, after one side has already been soldered in place, the other side lifts up, causing the component to stand at an angle on the printed circuit board. The chip then resembles a gravestone, which is why this fault is known by this name. Manhattan effect
Gram equivalent
Synonymous with the chemical equivalent (val). A specific quantity of an element or compound derived from the substance’s reaction behaviour (expressed in grams). In the case of flux, for example, this corresponds to the equivalent of acids or bases, or to the amount of acid containing 1 val of hydrogen acting as an acid, or to the base required to neutralise this amount. For RMA and RA fluxes, the relevant value is specified in the MIL standard. The unit is meq./g, where ‘eq’ stands for ‘equivalent’.
Basic grid
The abbreviations AGW and PEL are commonly used.
PEL values for soldering
metal vapours (as oxides) PEL (mg/m³)
Cd 0.100
Be 0.002
Zn 5.000
Sb 0.500
As 0.010
Pb 0.050
In 0.100
Ag 0.010
PEL values for soldering
This entry is based on the limit values applicable in the USA.
Such limit values exist, for example, for the concentration of metal vapour or metal dust in the air at the workplace. The measurement is the mass of metal vapour (mg) per cubic metre of air. OSHA specifies the above limit values for soldering. The amount of metal in the air is also referred to as airborne metal concentration.
Gull-wing lead
As electronic components have become smaller, the connection pins have also had to be designed to take up less space. To this end, they are often no longer inserted into holes, but are bent into a J-shape so that they form overlapping connections on the circuit board. This type of connection increases the reliability of the solder joint. Because this J-shape resembles the wings of a gull, it is known by this name. However, caution is advised: if mechanical stress remains within the pin, there is a risk that it will lift away from the circuit board due to the heat input, resulting in a faulty solder joint.
Halide
Compounds containing halogens, i.e. the elements of Group 17 of the periodic table (F, Cl, Br, I, At), namely fluorides, chlorides, bromides, iodides and astatides. The first three in this list are frequently used as activators for fluxes. Compounds between halogens are called interhalogens, whilst compounds of halides with the same or different halogens are referred to as polyhalides. Polyhalides are represented by formulas such as MXn; MXmYn; MXlYmZn, where X, Y and Z are different halogens and M is an alkali metal or ammonium, etc.
Halogen
An umbrella term for the five elements fluorine (F), chlorine (Cl), bromine (Br), iodine (I) and astatine (At) from Group 17 of the Periodic Table (IUPAC convention). The name ‘halogens’ is derived from the ancient Greek words for ‘salt’ and ‘to form’, as these elements form classical salts particularly readily with metals. Halogens are commonly used as activators in fluxes, as they facilitate the bonding of tin-lead solders with copper and lead-free alloys as the base material. The most abundant halogen in nature is chlorine, followed by fluorine, bromine and iodine. The radioactive element astatine occurs only in very small quantities. The halogens are similar in their properties – their melting point, boiling point and specific gravity decrease from fluorine to iodine. As the halogens have one fewer electron than the noble gases, their electron affinity is greater and they form monovalent ions more readily. They therefore form ionic bonds with strongly positively charged elements, whilst with negatively charged elements they form electron-pair bonds. The properties of the halogens are shown in the table.
Properties of the halogens
Element Fluorine Chlorine Bromine Iodine
Atomic number 9 17 35 53
Atomic mass 18.9984 35.453 79.904 126.9045
Melting point (°C) -217.9 -100.98 -7.3 113.7
Boiling point (°C) -188 –34.07 58.8 184.5
Critical temperature 144 144 311 Density
(g/l) 1.71 (0 °C) 3.22 (0 °C) 5.48 (87 °C) specific
gravity 1.109 1.571 3.14 atomic radius
(A) 0.71 1.01 1.14 1.34
Permittivity 1.517 (83.21 K) 1.94 (10 °C) 3.12
Physical properties of the halogens
Brazing
In brazing, a filler material (with a lower melting point) is inserted between two workpieces. The brazing gap is then filled with the molten filler metal by simultaneously heating the workpieces and applying pressure, thereby creating a joint between them. Borax is a suitable flux for this process. Depending on the brazing temperature, a distinction is made between soldering (up to 450 °C) and brazing (450 °C and above). In English, the terms ‘soft brazing’ and ‘hard brazing’ are used for this, although it could be argued that ‘soft brazing’ and ‘soldering’ essentially refer to the same process. Brazing is used, for example, to attach a tip made of tungsten carbide (an ultra-hard alloy) to a shaft (steel containing 0.7 % C). To secure a joint between two iron pipes, a liquid copper brazing alloy is applied to the outer surface, which rises into the gap between the two pipes due to capillary action. Dr C. J. Thwaites of the International Tin Research Centre in England therefore takes the view that soldering and brazing are not distinct technologies, but rather instances of what he terms ‘capillary joining’, as both make use of capillary action. German linguistic usage suggests a similar perspective.
Hot-air tinning (hot air levelling)
In this process, a rigidly mounted printed circuit board is immersed in a solder bath to coat its exposed surfaces with solder. Once the printed circuit board has been removed from the solder bath, two hot-air knives are directed at it; these blow away the excess solder using air at a temperature above its melting point. This process also cleans the through-holes and distributes the tin or tin/lead layer evenly across the printed circuit board, resulting in a smooth surface.
Heating element (heater)
As soft solders have a low melting point, they are often melted using natural gas. However, precise temperature control is difficult in this case and can be achieved more effectively using heating elements. The table below lists the most common heating wires and their chemical composition.
chemical composition of heating wires
Chemical composition Specific resistance (20 °C) µΩ cm Maximum operating temperature (°C)
Name Ni Cr Al Mn C Si Fe
Nichrome Type 1 75–79 18–20 <2.5 <0.15 0.5–1.5 <1.5 108 ± 7 1100
Nichrome Type 2 >57 15–18 <3.0 <0.20 0.5–1.5 Balance 112 ± 7 900
Iron-chromium
Type 1 23–26 3.5–5.5 <1.0 <0.15 Balance 140 ± 8 1200
Iron-chromium
Type 2 17–21 2–4 <1.0 <0.15 Balance 122 ± 7 1100
Chemical composition of heating wires
Heterogeneous material interface (heterojunction)
A bond at the atomic level between two or more different substances when joining different materials. This also includes the material bond formed during soldering. In contrast, the P-N junction in a silicon semiconductor, for example, is a homogeneous material bond, as it involves a bond between atoms of the same type.
Jet wave soldering
As the image shows, in this process the molten solder is blown onto the printed circuit board at a flow velocity of 2 m/s. This makes use of the Bernoulli effect in flowing liquids, i.e. the higher the flow velocity, the lower the pressure on outwardly curved surfaces, or on the outer surface of the solder stream. Consequently, the solder can completely cover the area around the component. Furthermore, as there is also a scrubbing effect from the uniform, rapid flow of solder, flux and gases generated by the jet can be removed more effectively. As shown, a cavity forms beneath the solder wave, which gives this process its name.
Hydrophilic radical
A radical in a molecule that forms bonds with water molecules particularly easily, e.g. the hydroxyl group OH, the carboxyl group COOH or the amino group NH. Flux becomes hydrophilic through the addition of polyoxyethylene. If the carrier substance of a flux contains a hydrophilic radical, its residues should be removed by cleaning with water.
Hydrophobic radical
A group within a molecule that forms bonds with water only with difficulty. These include copper alkyl (CuH₂n+1) or phenyl (C₆H₅) and other hydrocarbon groups. Owing to their low reactivity with water molecules, such compounds are used in NoClean fluxes, the residues of which do not need to be removed. Groups that readily bond with water are referred to as hydrophilic radicals.
Ionic bond
A chemical bond between ions of opposite charges formed by electrostatic attraction. In NaCl, for example, an electron transfer takes place between the metallic element (Na) and the non-metallic element (Cl), causing the former to become a cation and the latter an anion. This results in a relatively weak bond.
Ionisation tendency
If metal M1 comes into contact with an electrolyte solution that already contains ions of a second metal, M2+, an ion-exchange reaction takes place according to the equation M1 + M2+ = M1+ + M2. The direction in which this reaction proceeds depends on the metals involved, the solvent and the concentration of the electrolyte. If M1 forms ions more readily than M2, the reaction proceeds from left to right, resulting in a sequence of metals based on their tendency to ionise – the redox series: K, Na, Ca, Mg, Zn, Cr, Fe(II), Cd, Co, Ni, Sn, Pb, Fe(II), H, Cu, Ag, Hg, Au. This property is utilised, for example, when iron filings are added to the effluent from a copper mine to precipitate the copper and recover it. In the above formula, M1+ corresponds to the copper ions dissolved in acid (H₂SO₄) and M2 to the added iron. Since Fe (II, III) lies further to the left in the series than Cu, the reaction proceeds in the opposite direction and the metal M1 (Cu) is obtained. The redox series reflects the tendency of metals to displace hydrogen from a dilute acid, i.e. to react according to M1 + H⁺ → M1 + H.
This is significant in soldering, as the process involves a combination of solder material and metallic base material. If this comes into contact with a dilute acid (e.g. through the dissolution of SO₂ contained in exhaust gases) or is exposed to high humidity, the tendency towards ionisation can lead to corrosion of the solder joint.
Ionograph
A device which extracts ions from flux or coating residues on printed circuit boards, etc., using a circulating rinsing fluid (75 % IPA, the remainder being pure water), and measures the conductivity of the ion-containing solution in order to determine the level of ionic contamination on the board. The rinsing fluid itself is first neutralised by an ion-exchange resin and is therefore capable of extracting even small quantities of ionised substances. The procedure is illustrated in the figure. The resistance can be a maximum of 10⁹ →cm and is converted by a microprocessor into an NaCl equivalence value.
If flux residues on the solder joint are exposed to high humidity, the ions still present in them can become active and reduce the surface insulation resistance (SIR), leading to faults and malfunctions in the assembly. Such faults are often caused by contaminants that are invisible to the naked eye or hidden beneath components, which are ionised by the moisture.
Like ‘Omegameter’, ‘Ionograph’ is a registered trademark of Alpha Metal.
IPA
Abbreviation for isopropyl alcohol (isopropanol). One of the two isomers of propyl alcohol (propanol). Boiling point: 82.7 °C, specific gravity (20 °C): 0.7887. It is obtained by the reduction of acetone and therefore yields acetone again upon oxidation. It is used, amongst other things, as a diluent and post-flux in soldering, as well as for cleaning. The second isomer, n-propanol, is a liquid with an alcoholic odour and is miscible with water in all proportions. Isopropyl alcohol, isomer, post-flux
Cold joint
A term used in practice to describe a solder joint that was subjected to movement or vibration before the solder had completely solidified. This results in the solder joint having a rough surface, and the solder joint is inadequate or mechanically unstable. To prevent the components from shifting as far as possible, rapid solidification – i.e. a short period during which the solder remains in a viscous (pasty) state – is essential, particularly when soldering in mass production.
KANIGEN coating (KANIGEN plating process)
The name of a chemical nickel-plating process (e.g. using Ni-P) developed by General American Transportation Co., which is widely used, amongst other things, for nickel-plating connecting wires prior to soldering. The name is a combination of the words ‘catalysis’, ‘nickel’ and ‘generation’. The chemical components are nickel sulphate, sodium hypophosphite as a reducing agent, alkyl hydroxy carboxylic acid as a complexing agent, and other specialised stabilisers. To adjust the pH value in accordance with the application conditions, NaOH or H₂SO₄, etc., are added. Chemical nickel plating is also possible by utilising the different ionisation tendencies of the metals; however, this has the disadvantage that the nickel layer is less durable.
→ Ionisation tendency
Capillary action (capillary joining)
Both brazing and soldering are joining techniques based on the capillary effect. Therefore, brazed and soldered joints can also be regarded as capillary joints between metals. The capillary effect is defined as follows: ‘If a capillary (a narrow tube) is immersed in a liquid, the liquid level inside the capillary either rises above the liquid level outside it or falls below it. If the liquid wets the tube, the level rises; otherwise, it falls.” (Dictionary of Physics and Chemistry, Iwanami Publishers). In soldering, the former case applies, i.e. the wetting of the capillary (in this case, the base material) by the liquid (molten solder). Naturally, the surface tension of the molten solder has a major influence here. Let h be the difference in liquid levels between the interior of the capillary and the surrounding liquid, r the radius of the capillary, ρ the density of the liquid, γ its surface tension, θ the contact angle and g the acceleration due to gravity. Then the following applies:
h = 2 r cos θ
γ ρ g ∴ γ = 2 r cos θ ρ g h
The surface tension of a solder alloy is extremely difficult to assess, as it depends on many factors – amongst other things, it is closely related to the contact angle θ and to the self-alignment of components during assembly. → Meniscus, self-alignment effect
Kauri butanol number
‘Kauri’ refers to the kauri tree, a tall tree species commonly found in New Zealand, from whose resin varnish is produced. The kauri-butanol value is derived by comparing the solubility of this resin in butanol with its solubility in other solvents, and correlates well with the solubility of rosin in various solvents. For example, rosin is highly soluble in trichloroethane, for which the value is 124. It is used primarily in the evaluation of solvents for flux cleaning. Also known as the kauri-butyrate factor.
Notch effect
If a body has a notch or crack at a particular point, or if its cross-section changes abruptly, this can become the starting point for rapidly progressing material failure, as mechanical stress is concentrated at that point. Although this is a universal phenomenon, its severity varies depending on the shape and material. This effect is particularly pronounced when the notched area is subjected to repeated loading.
Kirkendall effect
If two flat metal surfaces are joined together and diffusion is induced at the interface by heating, the interface shifts due to the migration of vacancies and interstitial atoms. This effect can also be observed in soldered joints. Diffusion via vacancies in the lattice can be demonstrated particularly in face-centred cubic and body-centred cubic metallic crystals. Such vacancies occur particularly at the interface and can combine there to form holes or pores (voids). These voids are known as Kirkendall voids and form very readily, for example, in solder joints between Cu and Sn, as the two elements have very different diffusion coefficients. If phosphorus and oxygen are present, they can accumulate at the interface and exacerbate the formation of voids. In this way, the solder joint degrades due to the formation of Kirkendall voids. The problems encountered when solder-coating phosphor bronze are also attributed to this phenomenon.
Kiss Cleaning
A cleaning method in which a brush soaked in cleaning solution rotates over the circuit board. This improves contact with the solder side (in the case of through-hole assembly) and allows flux residues to be removed effectively. Although the removal of flux residues – or cleaning in general – should normally be avoided, as this can damage the assembly, in this method the cleaning solution does not come into contact with the components, meaning that even relatively inexpensive and strong chlorine-based cleaners can be used. Alcohol-based solutions cannot be used unless the components are specifically designed to be corrosion-resistant. In the final step, cleaning is carried out using a wave generated by a pump. As cleaning with this method is carried out in a very short time, the chemical energy of the solvent must be enhanced as far as possible by rapid rotation of the brushes and high pressure. If the cleaning time is altered, an evaluation of the results over several months is necessary to ensure the solvent is correctly calibrated, which is a disadvantage of this method.
Rosin (colophony)
A resin used in fluxes. To obtain it, the turpentine contained in the balsam of conifers is distilled to separate out the volatile turpentine oil, leaving pure resin behind. Its constituents vary greatly depending on the species and origin of the wood. In any case, however, rosin is a yellow-brown, porous solid containing abietic and pimaric acids, which is insoluble in water but highly soluble in alcohol, ether and benzene. It softens at 80 °C and melts at 90–100 °C. → Rosin
Rosin flux
Flux containing rosin (coniferous resin) as its main component, as well as activators. These include R and RMA fluxes. Recently, the solids content – that is, the percentage of solid rosin – has often been viewed as problematic, as a high solids content makes cleaning after soldering more difficult. Consequently, there is a demand for fluxes with the lowest possible solids content.
Conjugate solution
If two solutions, A and B, are mixed, it may happen that they dissolve into one another only to a very small extent and therefore form two separate layers. When two saturated solutions coexist in this way, this mixture is referred to as a conjugate solution. This applies, for example, to mixtures of ether and water, and water and phenol.
Grain boundary (crystal boundary)
When a molten metal is allowed to solidify, a large number of grains (crystallites) are initially formed, which then continue to grow radially until they eventually come into contact with one another. At this point, crystallisation is complete. The boundaries between adjacent grains are called grain boundaries. For this reason, metals are also referred to as polycrystals. The illustration shows this crystal growth. As the grain boundaries solidify last, impurities accumulate here, making them the weakest points in a metal’s structure. Fractures usually occur here. The zone melting process makes use of this phenomenon.
Grain size
Finer grain boundaries automatically result in smaller grains or crystallites. This property describes the grain size. The smaller the grain size of the alloy after soldering, the higher the strength of the solder joint generally is. Creep strength is also generally proportional to the square root of the grain size. Grain size depends on the cooling rate, the degree of deformation, the heating of the metal and other conditions, and can be specified as a relative value by observing the grain diameters under a microscope.
Grainy solder joint (alligator skin)
If a solder joint or solder cone cools very slowly, this can lead to significant grain growth, resulting in a rough, uneven surface on the solder. This is referred to as a grainy solder joint. As the surface reflects light less well and lacks a shine, it is also referred to as a dull solder joint.
Covalent bond
A type of bond in which two atoms share a pair of electrons. To indicate this, the single C–H bond or the double C–C bond are often written as C:H and
C :: C respectively. For this reason, the term ‘electron pair bond’ is also commonly used. Where there are multiple covalent bonds, the atomic distance decreases and, accordingly, more energy is required to break these bonds. The diagram shows the electron pair bonds in ethane (C₂H₆) and ethylene (C₂H₄). The former has one covalent bond (2 electrons), the latter two (4 electrons). With a distance of 1.3 Å (Ångström) between the carbon atoms, the bond in ethylene is shorter than that in ethane (1.5 Å) and is therefore more stable.
The compound becomes even more stable when both electrons in the pair have opposite spins. The thermal dissociation energy acting on an organic flux during soldering is relatively low, as the process takes place at a relatively low temperature. Therefore, when selecting the flux activator, the presence of covalent bonds and the number of electron pairs must also be taken into account.
Creep
Creep is the deformation of a workpiece that is subjected to a comparatively low stress over a prolonged period. As the diagram shows, creep is divided into three stages.
Stage 1: Deformation occurring within a short period of time.
Stage 2: Relatively slow-progressing deformation.
Stage 3: Sudden deformation leading to fracture of the workpiece.
As Sn-Pb solder alloys have a low degree of recrystallisation, they exhibit creep deformation even at room temperature. At elevated temperatures, this phenomenon becomes even more pronounced. Adding small amounts of Cu and Sb to the alloy makes it less susceptible to creep. The stress on the creep curve that leads to fracture of the workpiece is referred to as creep strength.
Heat of crystallisation, heat of solidification
Heat released when a substance changes from the liquid to the solid state whilst its temperature remains constant. Conversely, a substance absorbs heat when it changes from the solid to the liquid state without its temperature changing. This latter amount of heat is called the heat of fusion and is equal in magnitude to the heat of crystallisation. From the variation in the heat of crystallisation in the cooling curves, it is possible to determine the temperatures at which phase transitions occur, and phase diagrams can be drawn up from these results.
Heat sink
In English, ‘sink’ refers to the kitchen sink and, more generally, to a place where something accumulates. The higher the integration density of LSI packages, the more waste heat they generate, meaning that their surface temperature can sometimes exceed 80 °C. Components or devices designed to absorb this waste heat are known as heat sinks. These can, for example, be metal plates beneath or on top of printed circuit boards, which absorb and dissipate the heat generated or stored by the components and the circuit board itself. AIN printed circuit boards have the advantage that they insulate whilst at the same time conducting heat well.
Copper welding wire
Copper-coated or copper-plated iron wire. If the lead wires of capacitors or resistors are made of pure copper, they can bend when inserted, slowing down the production process, particularly in the case of automated assembly. Lead wires with an iron core are stiffer and easier to insert.
Copper mirror test
A widely used test method in accordance with JIS-Z-3197 (1986), Section 6.6.2. (IPC J STD 004 Test Method IPC TM 650 2.3.32), used to test the corrosive effect of fluxes for cored solders and solder paste, as well as liquid, solid and rosin-based fluxes, on a copper plate. For this test, a 1.0 × 25 × 76 mm glass microscope slide is cleaned and coated with a layer of copper, which should have a transmittance of 10 ± 5 % for visible light with a wavelength of 5000 Å. Flux for cored solder is dissolved in isopropyl alcohol (35 %) for testing. Subsequently, 0.05 ml of the solution is dripped onto the sample, which is then placed within 5 minutes into a container maintained at 23 ± 2 °C with a relative humidity of 45–55 %. After 24 hours, the residual flux is removed from the specimen using isopropyl alcohol, and it is compared with a reference specimen which has been treated with WW rosin flux dissolved in 35 % isopropyl alcohol. Corrosion is compared by visual inspection, with the aid of diagrams such as those shown below. To test solder paste or liquid flux, the flux to be mixed with the solder paste, or the undiluted product, is brought into direct contact with the copper plate, and the procedure is otherwise carried out as described above. A flux has passed the test if the vapour-deposited copper layer remains completely unchanged.
Litmus paper
Litmus paper
Filter paper impregnated with a violet colour pigment (actually a mixture of several pigments), which is obtained from dyer’s lichen and other species of lichen. As test paper, it provides a simple way of determining whether a liquid is an acid or a base: if red test paper is dipped into an alkaline liquid, it turns blue; if blue test paper is dipped into an acid, it turns red. The colour change occurs within a pH range of 5.0–8.0. If no colour change takes place, the solution is neutral and has a pH of 7.
Shelf life
Prolonged storage causes the soldering properties of solder paste to deteriorate. On the one hand, this is due to the high degree of mixing between the solder powder and the flux (liquid): because of the surface activation energy of the tiny solder particles, a chemical reaction between the components begins even during storage, and as a result, some of the activity of the solder surface is lost. On the other hand, the thixotropy of the flux also plays a role. It is therefore essential to ensure the shelf life of the solder paste. This period is also referred to as the shelf life of the solder paste.
Laser
The word ‘laser’ is an acronym formed from the initial letters of ‘light amplification by stimulated emission of radiation’. When concentrated laser beams are directed at a solder joint, the light is absorbed by the metal and converted into heat energy, causing the temperature of the solder joint to rise. This technique is particularly suitable for selective soldering, as the light can be easily focused onto a single point.
Latent heat
The amount of heat released or absorbed during phase transitions such as solidification, melting or evaporation, without any change in the temperature of the substance. The sensation of cooling that occurs when water is sprinkled on the ground on hot days is also due to the fact that the evaporating water extracts this latent heat from its surroundings. By measuring this change in heat, the phase transition temperatures of a substance can be determined.
Conductive resin
Generally, an epoxy resin adhesive to which copper or silver powder has been added in a volume ratio of 90 % or more. It is used as a substitute for solder to attach chips or LSIs and is particularly necessary for bonding a chip with an ITO electrode to a glass or plastic substrate (using pressure) or for manufacturing printed circuit boards with low heat generation. The areas where the adhesive has been applied are referred to as ‘bumps’.
Limonene
C10H16. A monocyclic monoterpene and derivative of p-menthane, which has a lemon-like odour. Main component of the cleaning agent EC-7, which AT&T (USA) markets as a substitute for the CFC cleaner CFC 131. Limonene occurs in two enantiomers, d and l, the former of which is contained in the aforementioned cleaner. d-Limonene is found mainly in bitter orange peel oil, lemon oil, bergamot oil and other citrus fruits, whereas l-Limonene is found in pine needle oil, peppermint oil, etc. The chemical structural formula of d-limonene is similar to that of abietic acid, which is found in rosin. As the limonene-containing cleaning agent EC-7 has a low flash point of 47 °C, the cleaning of the assemblies after soldering must be carried out in a nitrogen atmosphere. After cleaning with EC-7, rinsing with water is necessary.
Liquidus line
When the melt of a eutectic alloy consisting of two metals, A and B, cools, the metal present in the greater proportion crystallises first. The temperature at which crystallisation begins is referred to as the liquidus line of A or B. The line obtained by plotting the liquidus temperature of a mixture – that is, the temperature at which it begins to solidify – as a function of its composition is the liquidus line of the mixture.
Local element (local cell)
If a metal or alloy is immersed in an electrolyte solution, and if the metal, alloy or solution is inhomogeneous, localised electrodes (anodes or cathodes) may form, between which a current flows, thereby forming a galvanic cell. These tiny cells are known as local elements. If, for example, a solder joint is exposed to an electrolyte solution, processing cracks in the solder alloy, internal mechanical stresses or irregularities in the composition, temperature or pressure of the solution can lead to the formation of local elements and, consequently, to corrosion of the solder joint. The corrosion of solder joints upon contact with raindrops (particularly in the case of acid rain) can be caused not only by the actual chemical reaction but also by local elements. However, this should not be equated with galvanic current.
→ Galvanic current
Solvent extraction
A method for extracting a specific substance from a sample, which involves placing the sample in a suitable solution and rinsing it with that solution. This method is also used for the chemical analysis of solder residues. In addition to directly dissolving the sample, it is also possible to make the substance of interest easier to extract by carrying out specific chemical reactions beforehand. To extract from a liquid, immiscible solvents and a separating funnel are used. With this method, it is advisable to use a low-boiling-point solvent such as alcohol, ether, benzene, ethyl acetate or chloroform.
Solubiliser
Surfactants and other so-called solubilisers are used as additives to solubilise liquids and solids that are poorly soluble in water, so that they form a thermodynamically stable solution. In soldering, they act as an additive to the flux carrier and prevent it from solidifying before cleaning. This enhances the effectiveness of the cleaner.
Fusible solder alloys
Chemical composition (%) Temperature (°C)
Bi Pb Sn Cd Other Solidus Liquidus
44.7 22.6 8.3 5.3 In 19.1 47 47
49.0 18.0 12.0 - In 21.0 58 58
48.0 25.63 12.77 9.6 In 4.0 61 65
50.0 26.7 13.3 10.0 - 70 70
42.5 37.7 11.3 8.5 - 71 87
55.5 44.5 - - - 124 124
58.0 - 42.0 - - 139 139
40.0 - 60.0 - - 139 170
48.0 28.5 14.5 - Sb 9.0 103 226
Solder alloys
Soldering
A method of joining two metal parts using a filler metal consisting of a metal or alloy with a lower melting point than the base materials, in which the filler metal is melted between the metal parts to be joined and forms a thin alloy layer on them, which helps to strengthen the joint. Generally speaking, soldering at temperatures below 450 °C is referred to as soft soldering, whilst at higher temperatures it is known as brazing. If the alloy layer becomes too thick during this process, the joint may come apart more easily; therefore, overheating or an excessively long soldering time must be avoided at all costs. As soldering is only possible through metal exchange at the atomic level, the material surfaces must be clean and metallic. Soldering is classified as a joining process and is often discussed in this context. Soft soldering and brazing are different joining techniques which are referred to by different terms depending on the language (see table).
Terms for soft soldering and brazing in various languages
Language Soft soldering Brazing
English soldering or soft-soldering brazing, hard-soldering
French brasage tendre / soudage tendre brasage (fort)
Dutch zachtsolderen hardsolderen
Italian saldatura dolce saldatura forte
Spanish soldadura blanda soldadura fuerte
Japanese handa-zuke r-zuke
Terms for soft soldering and brazing in various languages
Soldering flux
With the exception of special cases (e.g. friction soldering, soldering in a reducing atmosphere, mechanical joining), flux is used in soldering to clean the joint, prevent oxidation of the metal and reduce the surface tension of the molten solder, thereby improving wetting. To this end, it must be capable of both removing surface oxides from the metal and bringing the solder into direct contact with the base material. To achieve this effect, rosin-based flux is usually used, also known as R-flux (where R stands for rosin). However, as high working efficiency cannot be achieved with this alone, activators are normally added to the flux in industrial applications. Assessing the effectiveness of a flux is extremely complicated, as, in addition to the solder material, factors such as the base material, the type and quality of the parts to be soldered, the conditions of the soldering process, the requirements for the solder joint, and the type and quantity of chemicals added to the rosin must all be taken into account. In fluxes intended for use in solder paste, for example, over 20 different activators may be present in some cases. The exact composition is a trade secret of the manufacturers and is not disclosed. To categorise fluxes according to their performance, the US military standard MIL uses the abbreviations R, RMA and RA, where RMA stands for ‘Rosin Mildly Activated’ and RA for ‘Rosin Activated’. Activators are essentially halides, and the classification into RA and RMA is based on their quantity. Residues from RMA fluxes contain comparatively few halogens, which is why cleaning is not required (NoClean fluxes).
Depending on the type and proportion of activators, a distinction can also be made between water-soluble and water-insoluble fluxes. Flux usually contains rosin or resin, in which the reaction products between the oxides of the solder and the base material and the activator dissolve, as well as a binder. The concentration and viscosity are adjusted to the soldering conditions by mixing with a diluent. However, as water-soluble flux is corrosive, the soldering process must be followed by a cleaning step consisting of rinsing with water and neutralisation. Water-insoluble flux exists in rosin- and resin-based forms and is very commonly used in the soldering of electronic devices. The R, RMA and RA fluxes listed in the table below fall into this category. RMA fluxes are subject to stricter regulations regarding the use of halogen-containing activators and may therefore remain as residues on the assembly without requiring cleaning. The second table provides an overview of the activators for water-soluble fluxes and the corresponding water-based cleaning processes. Suitable binders for such fluxes include glycerine, polyethylene, glycol, polypropylene, glycol-polyoxyethylene or phenyl ether; suitable diluents include water, alcohols with a carbon number of 1–3 or high-boiling-point alcohol ethers. As Table 3 shows, water-insoluble flux consists of rosin or resin with activators; however, cleaning with water is also possible, particularly where the solids content (rosin content) is 5 % or less. Diluents such as terpenes, alcohols with 1–4 carbon atoms, and others are used for this purpose. The fluxes mentioned above are primarily suitable for pre-flux or post-flux applications, whilst solder paste fluxes have a different composition. Typical fluxes of this type are listed in Table 4. The test specifications for such fluxes can be found in the Federal Spec. (QQ-S-571E).
Specifications from the MIL standard on flux performance (MIL-F-14256E)
Type Halide content in mval/g of the solid product Resistivity of the aqueous extract
(Ω·cm)
Copper mirror test Surface insulation resistance (MΩ) Solder spread (mm)
R 0.00 >100,000 no removal > 100 -
RMA < 0.040 > 100.00 as above as above > 90
RA < 0.284 > 50,000 - as above > 100
Specifications from the MIL standard on flux performance (MIL-F-14256E)
Chemicals contained in water-soluble flux and methods for cleaning it off
Application Chemicals Cleaning methods
Printed circuit boards for domestic electronics inorganic salts of amines or amino acids: methylamine or glutamic acid hydrochloride, pyridine hydrobromide, etc. removal of residues using tap water or demineralised water
Printed circuit boards for industrial equipment organic salts of amines and amino acids: glutamic acid oxalate, dimethylamine succinate see above.
Pre-soldering of electronic components and soldering of printed circuit boards organic acids: glycolic acid, lactic acid, malic acid, citric acid, formic acid, acetic acid, oxalic acid, malonic acid, succinic acid, etc. First clean with hot water, then treat water-insoluble residues with 2 % HCl and neutralise
with water General applications inorganic acids: hydrofluoric acid, hydrochloric acid, hydrobromic acid, hydroiodic acid, tetrafluoroboric acid, phosphoric acid, etc. Clean with hot water and neutralise
with an alkaline solution. Tin plating or tin/lead coating of thin copper plates Inorganic acids: zinc chloride, ammonium chloride, sodium chloride, stannous chloride, sodium fluoride, etc. After tin plating, clean with hot water and neutralise
with an alkaline solution. Chemicals contained in water-soluble flux and methods for its cleaning.
Chemicals
contained in water-insoluble flux. Application Chemicals:
Soldering of printed circuit boards for industrial equipment and soldering of silver electrodes Rosin-based – organic acids or organic salts of amines;
soldering of printed circuit boards for domestic electronics rosin-based – organic acids, organic salts of amines, amine halide salts
heavy-duty solder joints in military equipment or satellites, and soldering of thin copper wire up to 0.5 mm in diameter abietic acid contained in rosin (rosin only)
Soldering of printed circuit boards for industrial equipment synthetic resin-based – organic salts or organic salts of amines
Soldering of printed circuit boards for domestic electronics synthetic resin-based – organic acids, organic salts of amines, amine-rosin salts
Chemicals
contained in water-insoluble flux Flux for solder paste
Function Ingredient Proportion in mixture (% by weight)
Rosin WW rosin 64
Solvent Butyl carbitol 30
Thixotropic agent Hydrogenated castor oil 5
Activator Ethylamine hydrochloride 0.5
Other organic salts (abietic acid) 0.5
Flux for solder paste
Solder dross
Oxidation products that settle on the surface of a melt are often referred to as slag. However, the term ‘dross’ encompasses not only the oxidised metal dispersed throughout the melt, but also deposits at the bottom of the melt. The term ‘sludge’ is also used in this sense. Sludge can, however, also refer to non-metallic waste, such as that produced during wastewater treatment. In addition, there is also the term ‘slime’. All these terms refer to waste and are often used without clear distinction. ‘Solder dross’ refers to the oxides of tin and lead produced when solder is melted.
Globule test
A test method in which a molten solder globule is placed on a surface that the solder does not wet (a glass or stainless steel plate), and a copper wire is lowered horizontally so that it divides the solder globule into two parts. Wetting is assessed on the basis of the time taken for the solder to envelop the copper wire. Although this method does not allow for quantitative measurement, it provides a quick qualitative indication of wetting.
Soldering oil
Oil added to the solder bath to protect the surface of the solder from oxidation or to reduce its surface tension so that it flows more freely. The main components are water-soluble oils or mineral oil; many products contain glycols. In wave soldering systems, the soldering oil is also fed into the solder bath by means of a pump. As the oil can be a source of contamination, the recovery of fluxes, oil, solvents, etc. must be taken into account in advance. In particular, care must be taken to prevent oil residues from causing disruptions in the cleaning process. As there are both advantages and disadvantages to its use, it is advisable to weigh these up carefully.
Solder sleeve connector
The term ‘solder sleeve’ is in fact a registered trade name of Raychem Co., Devices Division (300 Constitution Drive, Menlo Park, California 9402). It is a technique in which several conductors, previously coated with flux and solder, are inserted into a heat-shrink tubing, which is then heated at the insertion point with hot air to over 125 °C, causing the tubing to shrink and the conductors to be joined. The illustration shows a longitudinal section of the heat-shrink tubing with the cable connection after processing.
Solder resist
A material used to coat areas that are not to be soldered, in order to protect them from contact with solder. The substances listed in Table 1 are used for this purpose. The majority of solder resist coatings are organic in nature. These include melamine-based coatings, which, although they have the disadvantage of producing toxic formaldehyde during condensation, are widely used in the manufacture of industrial printed circuit boards due to their low cost. UV-curing solder resist, on the other hand, has poorer coating properties but is used in printed circuit boards for domestic electronics due to its good processability. Table 2 shows the various types of solder resist and their properties.
Types of solder
resist:
organic thermosetting (epoxy/melamine-based), inorganic aluminium oxide powder, graphite powder, magnesia powder
Types of solder
resist Properties of various solder resists (epoxy=100)
Property
Resin Insulation Heat→resistance Solvent→resistance Dielectric strength Adhesion
Epoxy 100 100 100 100 100
Melamine 100 60 50 50 60
UV-curing 100 60 50 80 60
Properties of various solder resist coatings (epoxy=100)
Solder icicle
A defect in which solder icicles form on solder cones or wire ends (see illustration). This frequently occurs when there is insufficient solder or when the diameters of the contact hole and the pin do not match. If the gap between the two is too small, the solder may flow out of the hole under its own weight and form icicles. When soldering by hand, the heat supplied by the soldering iron is often insufficient. In this case, a more powerful soldering iron or a tip with a larger contact area should be used.
Air knife
A compressed-air nozzle used to remove excess solder from a printed circuit board once it has been removed from the solder bath following wave soldering. This revolutionary invention is used in many soldering processes. The name ‘knife’ originated because the compressed air slot resembles the blade of a knife.
Marginal solderability
The condition under which soldering is just about possible. As wetting or non-wetting, as well as de-wetting, play a role here, it is difficult to assess this by visual inspection alone, and testing with a wetting balance is preferable. In this context, the term ‘marginal wetting’ is also used.
Matrix effect
According to the Duden Dictionary of Foreign Words, ‘matrix’ is Latin for ‘female parent’ or ‘origin’. In chemistry, the term refers to a carrier substance into which other substances integrate or become embedded. For example, if chemical products or reaction residues are removed using a solvent in which they do not actually dissolve well, the solvent can nevertheless penetrate the surface of the compounds to be removed and wash them away as part of a larger solution complex. This is known as the matrix effect. In soldering, this effect occurs when one attempts to remove the tin, lead or other metal salts formed from rosin using a strong solvent.
MCM (Multi-Chip Module)
A multi-chip module is usually defined as a module containing several bare semiconductor chips. However, the term is also used for components in which a multi-layer thin-film circuit is formed on a substrate and populated with LSI bare chips. These components are soldered. Also known as MCP (Multi-Chip Package).
Meniscograph (meniscographic method)
Apparatus for measuring the forces exerted on a test specimen (base material) by buoyancy and surface tension when it is immersed in a solder bath. As the temporal behaviour of wetting depends on the flux and the material, an analysis of the measured wetting curve allows for a quantitative assessment of solderability. → Wetting balance, wetting rate
Meniscus
If a liquid (liquid solder) is poured into a tube, its surface curves either upwards (convex meniscus – Fig. a) if the liquid does not wet the tube wall, or downwards (concave meniscus – Fig. b) if wetting occurs. In this way, the wetting of a base material by a solder can also be investigated.
Webbing
Refers in particular to small droplets or strands of solder on insulated areas of the printed circuit board or between the metal connection pads. The irregular shape, compared with ordinary solder joints on circuit boards, is due to the smaller amount of flux.
There are essentially four causes of ‘webbing’:
incorrect curing of resins in multilayer printed circuit boards or of solder resist on the board
rough surfaces due to excessive friction, corrosion caused by solvents or unsuitable solder resist
Beading of dross upon contact with the printed circuit board due to insufficient flux
generally due to a lack of flux. To prevent this, it is advisable to determine the density and flow rate of the flux in advance.
Non-wetting
Unlike in the case of de-wetting, this involves a surface that has not been wetted by the solder at all. This is easily recognised during soldering by the fact that the colour of the base metal has not changed. In this case, the contact hole cannot be filled with solder and the gap between the pin and the hole wall is too large, meaning that the solder joint is considered incomplete.
Nitrogenius
Brand name of a wave soldering system developed by Seho (Germany), in which the soldering process takes place in a nitrogen atmosphere. The unit is gas-tight and ensures a residual oxygen concentration of no more than 10 ppm, which prevents the solder from undergoing oxidisation during the soldering process. Formic acid is sometimes added to the nitrogen gas; as it contains an aldehyde group, it acts as a reducing agent. At 160 °C, it decomposes into carbon dioxide (CO₂) and hydrogen, which enhances the reducing effect.
Levelling
Removing excess solder from a solder-coated printed circuit board that has tarnished during storage or requires reworking, by melting the solder and blowing it off with air or removing it using centrifugal force. When air is used for this purpose, the process is known as hot-air levelling or hot-air tinning.
Nocolok process
A process for brazing aluminium, developed by the Canadian company Alcan. A eutectic alloy consisting of the potassium fluoroaluminates K₃AlF₆ to KAlF₄ is used as the flux; its behaviour corresponds to the phase diagram of the binary AlF₃–KF system (AlF₃ 44 %, KF 56 %, eutectic temperature 562 °C). The brazing process takes place under a protective N₂ gas or in an atmosphere with a low dew point. In its molten state, the flux is highly active, whilst at room temperature it is completely inactive. This eliminates the need for cleaning after brazing. The name ‘Nocolok’ is easy to remember if you think of ‘Nocolor’, referring to the colour remaining unchanged after brazing.
OA flux
Water-soluble fluxes that have been strongly activated with amines of organic acids or hydrochloric acid. In the electronics industry, organic substances and acids are frequently used in combination, and these fluxes are therefore widely used in both water-soluble and water-insoluble forms. OA = abbreviation for organic activated fluxes.
Surface tension
Liquids (including molten metals) tend to minimise their surface area as much as possible and, were it not for the influence of external forces, would assume a shape approximating that of a sphere. This property is known as surface tension. It is based on the attractive forces between the molecules of the melt, which manifest themselves as tension at the surface. Surface tension corresponds to the work required to increase the area of a molten metal by one unit whilst maintaining a constant temperature, and is identical to the Gibbs free energy stored per unit area. In soldering, this phenomenon affects the interface between a liquid and a gaseous phase (air); however, surface tension also occurs at liquid–liquid, solid–liquid and solid–solid phase boundaries, provided that the change in surface area is accompanied by an energy transformation. In principle, surface tension is the result of the interaction of attractive forces between molecules within the respective phases and at the phase boundary; in practice, however, only the surface tension of the melt can be measured. It is determined according to S. Sugden (S. Sugden: J. Chem. Soc., 1922, 121, 858). The measurement of the surface tension of solder using this method is described, for example, by M. A. Carroll, M. E. Warwick, I.T.R.I. Pub. No. 690 as follows: Gas bubbles (argon) are introduced through a tube of radius r, which is immersed to a controlled depth h in the molten metal (solder). The gas pressure initially creates a small gas bubble with a relatively large radius of curvature, which then grows into a hemispherical bubble with the same radius as the tube. Under continued pressure, the bubble grows larger and larger until it detaches from the tube and bursts. Consequently, the highest pressure at which the bubble remains stable is that at which it has the smallest radius. The following equation applies to this maximum pressure:
Pmax = 2γr + gh (ρ1 – ρ0)
where γ is the surface tension, ρ1 and ρ0 are the respective densities of the melt and the gas, and g is the acceleration due to gravity. The figure shows the relationship between surface tension and the temperature of the solder, as measured in this way. As a general rule, surface tension decreases as the temperature rises. It is also dependent on the chemical composition of the material in question. The decrease in surface tension as the temperature rises is due to changes in the thermal motion of the molecules. During soldering, the effect of the surface tension of the cooling solder causes components to self-align on fine-pitch printed circuit boards. Examples of the surface tension of various substances in air, expressed in dyn/cm, include water at 72.75 (20 °C), mercury at 487 (15 °C) and ethyl alcohol at 22.3 (20 °C). → Gibbs free energy, self-alignment effect.
Omegameter
A device which washes out ionic residues from SMD circuit boards using a rinsing liquid and subsequently determines the ionic concentration on the circuit board by measuring the electrical resistance of the liquid. The rinsing liquid consists of isopropanol (75 %) and pure water. The circuit board is immersed in a solution heated to 50 °C and then subjected to a high-pressure jet to maximise ion uptake. A microprocessor converts the measurement results into an NaCl equivalence value. Registered trademark of Alpha Metal.
Orange peel effect (crinkling)
If the solder resist is applied to the printed circuit board after tin plating, heat may not be dissipated effectively, causing individual areas to overheat and the tin layer beneath the solder resist to melt. This causes the solder resist to warp and form creases, a phenomenon also known as ‘orange peel’. The reason for this phenomenon is the relationship between the internal stress of the solder resist and the cohesive force of the solder.
Passivation (passivity, passive state)
When passivated, common metals behave in a similar way to precious metals. Iron, for example, dissolves in a dilute nitric acid solution, but not in a concentrated one. Once iron has been immersed in a concentrated nitric acid solution and is subsequently immersed in a sulphuric acid-copper solution, no precipitation of iron occurs through substitution with copper. The reason for this is that a thin oxide layer has formed on the metal, completely covering it. This so-called passivation usually takes place immediately if the solution into which the metal is immersed contains a sufficient amount of oxidising agent. In this case, the process is referred to as self-passivation. Stainless alloys are often self-passivating. Therefore, care should be taken to remove the passivation layer beforehand when soldering.
pH value (hydrogen ion exponent)
The pH value, a measure of the concentration of hydrogen ions in an aqueous solution, is defined as follows:
pH = -log₁₀ [H⁺]
where [H⁺] is the molar concentration of hydrogen ions (mol/dm³). At 25 °C, in a neutral solution, [H⁺] = [OH⁻] = 10⁻⁷ mol/dm³, therefore neutral solutions have a pH of 7. If the pH is below this, the solution is an acid; if it is higher, it is a base. Nowadays, relative activity (aH) is usually used instead of molar concentration.
Phase rule
Also known as Gibbs’ phase rule, as it was formulated by J.W. Gibbs (1839–1904). For thermodynamic equilibrium to prevail in a heterogeneous system (multiphase system), the chemical potentials of the substances in the system must be equal. Let p be the number of phases in the heterogeneous system and c the number of substances. Then the following applies:
f = c – p + 2
Here, f is the number of degrees of freedom (independently variable state variables).
If the system consists of only one substance (c = 1) present in liquid, solid and gaseous forms (p = 3), then f = 0, i.e. temperature and pressure are fixed. If the system is of a solid nature and the pressure is constant, there is one fewer degree of freedom and the following applies: f = c – p + 1.
During the actual soldering process, the diffusion zone is not a system at equilibrium and the phase rule therefore does not apply in this form. However, it does apply to the solder itself.
Polishing (buff polishing)
To polish metal samples for microscopy, a cloth that is largely free of protruding fibres is stretched over a polishing disc, in front of which the sample is positioned vertically. Whilst the polishing disc rotates, a polishing compound consisting of aluminium oxide (Al₂O₃) mixed with paraffin or a similar substance, or diamond grains approximately 6 µm in size, is applied to the surface. ‘Buff’ refers here to a leather-covered high-gloss polishing disc. Particularly when preparing microscopy specimens from soft solder, care must be taken not to apply too much vertical pressure to the specimen, as this would cause the surface layer of the metal to shift, preventing the actual structure from being revealed. To prevent overheating, a sufficient quantity of polishing compound must always be applied to ensure that the solder does not recrystallise.
Polymer rheology
Polymer rheology deals with dispersions and suspensions as viscous systems; that is, liquids in which solid particles are dispersed. The latter also include solder paste as well as commercially available inks and paints. Solder paste is a suspension consisting of a binder (vehicle) and solder particles. Coating agents for paper are also suspensions comprising a polymer solution into which solid particles of clay and other materials are mixed.
Pore (vacancy, void)
An empty space in the crystal lattice of a crystal where no atoms are present. As a so-called vacancy, it is classified as a crystal lattice defect. Vacancies can migrate within the crystal lattice, pair up to form double vacancies, or form crystal pores consisting of several vacancies. Not to be confused with blowholes, which are caused by gas escaping from molten metals.
→ Kirkendall effect
Pre-Flux
A flux applied prior to post-flux treatment, which is applied to the freshly etched copper circuit pattern to prevent oxidation. If post-flux treatment is subsequently carried out, it is essential to ensure that the fluxes are thoroughly replaced. To ensure optimum coverage by the flux, it should have a high viscosity, with the molecular weight and softening point of the rosin and activators it contains playing a major role. This is known as the flux’s coverability.
Pre-cutting
Trimming the lead wires of components prior to assembly in through-hole mounting, in order to standardise the wire lengths. The process steps are usually precutting → shaping → soldering → cutting, although cutting at the end should be avoided where possible. Trimming the leads again after soldering can have undesirable consequences, such as: 1.) cracks in the solder joint, 2.) exposure of the iron wire ends, making them susceptible to corrosion, 3.) damage to components.
PS soldering process
PS is the abbreviation for Pressure Soldering. It is a pressure soldering process that offers two advantages: 1.) No flux is required, 2.) No porosity. It was developed by Tokuda, Chiba and Mizuishi at the Hitachi Research Centre and will be explained here using the example of a silicon pellet being soldered onto a substrate (see figure). To do this, the contact surface is first metallised.
(1). The Si pellet is placed on the substrate with a pre-formed solder deposit acting as an intermediate layer. The ambient pressure is then reduced to P1 (approx. 1 Torr). As there is naturally a gap at the contact surface, the pressure P1 also prevails inside the solder preform.
(2). When the solder melts, the gap disappears and the interior of the solder preform is hermetically sealed at P2.
(3). When the external pressure is then restored to standard pressure P2 (760 Torr), a pressure difference (P2–P1) arises between the interior—which was hermetically sealed at P1—and the exterior, causing the molten solder to flow immediately into the cavity of the solder preform.
(4). The heat supply is interrupted and the solder solidifies.
If we denote the volume and temperature inside the solder preform at the time of steps (2) and (4) as V1, V2, and T1, T2 respectively, then Boyle’s and Charles’s law gives:
Pycnometer (specific-gravity bottle)
A measuring vessel used to determine the specific gravity of a liquid. In the quality control of soldering flux, it is used in the factory to easily measure specific gravity. It consists of a glass bottle with a stopper through which a vertical capillary (narrow tube) passes, open at both ends. The vessel is filled, the stopper is inserted, and any liquid overflowing from the stopper is removed. The temperature and weight of the liquid in the vessel are then measured.
If the pycnometer has a mass of w when empty, a mass of W when filled with water, and a mass of W’ when filled with the test liquid, the specific gravity of the liquid is given by:
W’ – w / W – w
R flux
A flux consisting solely of rosin and solvent, without an activator. It is used particularly in applications requiring a high degree of reliability, such as with IC components. For soldering lead wires, a flux consisting of 25 % coniferous resin and 75 % isopropanol (IPA) is generally used. The following specifications apply: water-extract resistance > 100,000 cm, SIR > 500 M.
RA flux
The initials RA stand for ‘rosin-activated’. This is a flux whose activity has been enhanced by adding relatively large quantities of an activator to coniferous resin. Amines or amine hydrohalides are usually used for this purpose. In the US military standard MIL-F-14256, colophony derived from balsam resin, root resin, tall oil resin or modified colophony is dissolved in a non-halogenated solvent, and the activator is added to this solution to improve wetting. The following applies: acid number (SZ) > 130, solids content > 51 %, solution resistance > 50,000 → cm, SIR (surface insulation resistance) > 500 M→ (2 hours after return to normal conditions following heating and humidification at 85 °C and RH = 85 %), solder spread > 100 mm² on a brass plate. In this context, the permissible halogen content (sum of F, Cl and Br) in 1 g of solids is 0.284 mval when titrated with 0.1 N silver nitrate.
Reflow soldering (reflow)
Originally, ‘reflow’ referred to the remelting of a layer of solder; nowadays, however, it is understood to mean the heating of a flux-solder combination that has previously been placed at the desired location in order to form a solder joint. As such, the meaning now differs very little from that of soldering itself (H.H. Manko: Soldering Handbook for Printed Circuit and Surface Mounting, p. 192). In surface-mount technology (SMT), far-infrared radiation is used to melt the solder in the reflow process, as this allows individual spots to be heated precisely without affecting the rest of the printed circuit board. The far-infrared radiation is normally generated by a heating element consisting of nichrome wire coated with ceramic (Fe₂O₃).
Cleaning sponge (wiping sponge)
Sponge for removing flux residues and solder dross from the tip of the soldering iron. When the hot soldering iron tip is cleaned with a damp sponge, water vapour is produced, which is why this process is also referred to as ‘steam cleaning’. These specialised sponges allow the copper tip to be cleaned effectively without damaging its thin iron coating. To collect excess solder and dross, cleaning sponges often have a cavity in the centre.
Clean room
A room in which the concentration of dust in the air, temperature, humidity and pressure are strictly controlled to ensure a high level of cleanliness. As the level of contamination from foreign substances during the manufacture of electrical equipment and components (semiconductors) must not exceed certain ppm values, production must take place in a cleanroom. The US standard FED-STD-209E (replaced by ISO 14644-1) defines cleanroom conditions as follows:
Cleanroom class Maximum number of dust particles larger than 0.5 µm per ft³ (per l) Maximum number of dust particles larger than 5 µm per ft³ (per l)
100 100 (3.5)
10,000 10,000 (350) 65 (2.3)
100,000 100,000 (3,500) 700 (25)
Cleanroom class according to
ISO 14644-1 Maximum concentration of dust particles up to 0.5 µm in particles per m³ Maximum concentration of dust particles up to 5 µm in particles per m³
100 – ISO 5 3,520 29
10,000 – ISO 7 352,000 2,930
100,000 – ISO 8 3,520,000 29,300
Recrystallisation occurs, for example, when a material has developed internal mechanical stresses as a result of cold working and is then annealed at a suitable temperature. This causes new grains to form from the original crystal grains, and the entire crystal structure of the material is renewed, thereby relieving the stress. The temperature at which this process begins is known as the recrystallisation temperature. It is usually about half the melting point of a metal. Tin, however, is an exception – tin recrystallises even below room temperature. Forming normally refines the grains of a crystal and causes internal mechanical stress to build up. Subsequent heating causes the atoms to vibrate until their kinetic energy reaches a maximum, at which point the crystal grains break down and form a fine structure. This relieves the internal stress. With further heating, grain growth resumes and the grain size increases as the temperature rises. Recrystallisation depends not only on the type of alloy, but also on the degree and nature of the working carried out prior to heating. If, for example, a material is heated to the recrystallisation temperature after relatively little forming, the grains sometimes grow very rapidly and form larger single crystals. A high level of internal stress is not strictly necessary to induce recrystallisation; a few per cent is usually sufficient. This method of recrystallisation by heating is also frequently used to produce single crystals from iron or nickel or their alloys. Solder alloys (Sn-Pb and similar) become softer through forming, however. This is due to the recrystallisation of tin even below room temperature. The stress generated during work hardening is immediately relieved by recrystallisation. This is referred to as work softening.
Relative ionic conductivity
When measuring ionic conductivity on a printed circuit board or in solder residues, the measured value is often converted to a sodium chloride equivalent value (NaCl = 1). This value corresponds to the conversion of the ionic concentration into the equivalent concentration of NaCl ions. The conversion factor is determined by defining the conductivity of NaCl ions at a concentration of 8.6 × 10⁻³ µg/cm³ as 1, reading off the corresponding concentration from the conductivity curves of other compounds, and expressing these concentrations as a ratio.
Relative ionic conductivity of foreign substances on printed circuit boards when NaCl = 1.0
Compound Molecular formula Relative concentration (µg → m⁻³)
Carbonic acid H₂CO₃ 0.16
Hydrochloric acid HCl 0.18
Sulphuric acid H₂SO₄ 0.24
Malonic acid HOOC·CH₂·COOH 0.27
Succinic acid HOOC·CH₂·CH₂·COOH 0.31
Calcium hydroxide Ca(OH)₂ 0.31
Caustic soda NaOH 0.35
Propionic acid CH₃.CH₂.COOH 0.40
Ammonium chloride NH₄Cl 0.72
Calcium chloride CaCl₂ 0.88
Sodium carbonate Na₂CO₃ 0.96
Sodium chloride NaCl 1.000
Potassium chloride KCl 1.02
Copper chloride CuCl₂ 1.12
Copper sulphate CuSO₄ 1.28
Lead chloride PbCl₂ 2.04
Relative ionic conductivity of foreign substances on printed circuit boards, where NaCl = 1.0
Resist
A coating material used in etching, in tin-lead coating, during the application of solder, and in wave soldering, with the aim of protecting circuit board components from oxidation caused by contact with the etching solution or the solder. There are different types of resist, such as photofoil (dry film resist or a three-layered foil comprising a support film, photosensitive plastic and a protective film), organic resists made from commercially available plastics (e.g. polyamide, polyethylene or urethane), or metallic masks. In metallic masks, a tin-lead coating is mainly used, but gold or rhodium masks are also manufactured. These are known as solder resists.
Rheology
When manufacturing and using solder paste, particular attention must be paid to the factors that determine its viscosity, as this property is of crucial importance both for printing solder paste onto printed circuit boards and for the homogeneous mixing of the solder powder with the flux. Theoretically, the motion of bodies exhibiting elastic behaviour can be described by Hooke’s law (1676) and, in the case of pure viscosity, by Newton’s laws (1685); however, the fluids encountered in practice are subject to both to varying degrees and must therefore be considered from both these perspectives. This analysis is the subject of rheology. The term ‘rheology’ derives from the Greek words ‘rhei’ (to flow) and ‘logos’ (study) and dates back to 1928. The behaviour of solder paste also falls within its scope.
Rheopexy
In contrast to thixotropy (the breakdown of a fluid’s structure due to shear forces and its subsequent restoration after a certain period of rest), rheopexy refers to the phenomenon whereby low shear forces promote the formation of structure within a fluid. This phenomenon, discovered by Herbert Max Finlay Freundlich (1880–1941), can be observed by filling a 1 cm-thick test tube with a thixotropic suspension consisting of 42 % gypsum particles measuring 1–10 µm, shaking it and then leaving it to rest. The mixture only sets after 40 minutes. However, if the test tube is slowly rotated about its axis between the palms of the hands, the gypsum sets in just 20 seconds – that is, in one-hundred-and-twentieth of the time. The reason for this is that the strong shear forces exerted during shaking destroy the structure of the fluid and transform it into a sol, whilst the relatively low force exerted during rotation accelerates its setting.
RMA flux
The initials RMA stand for ‘rosin mildly activated’. The amount of activator added is lower than in RA flux, which is why the assembly can be processed further without cleaning after soldering. Also known as a weakly activated flux. The MIL-F-14256 standard specifies the following limit values, which differ from those for RA flux: solution resistance > 100,000 → cm, SIR > 500 M → solder spread > 90 mm² on a brass plate, halogen content < 0.040 mval (measurement conditions as for RA flux). RMA flux is also increasingly being used in solder paste.
Rosin
Also: colophony. Resin that remains after the volatile turpentine oil has been separated by distillation from the turpentine secreted by coniferous tree trunks. Its main constituents are abietic and pimaric acids, although the composition varies depending on the plant species. Colophony is a yellow-brown, crumbly substance that dissolves readily in alcohol, ether and benzene, but not in water. It softens at 80 °C and melts at 90–100 °C. As the temperature rises further, gases and pinolin are released, and at temperatures above 230 °C, approximately 60–80 % of the rosin oil is distilled off. Pinolin is used as a substitute for turpentine oil, whilst rosin oil is used in lubricants.
Haloing
To improve the adhesion of internal conductor patterns in multilayer printed circuit boards, the copper is pre-treated by oxidation to form a black oxide layer. However, this black oxide layer can be attacked by the hydrochloric acid used to metallise the drill holes, i.e. it can be reduced and detached. This results in a whitish or reddish copper oxide ring forming around the via, known as a ‘red ring’ or ‘pink ring’. This phenomenon is also referred to as red ring formation or ‘haloing’. This reduces the adhesion of the inner layers. In standard circuits, the effects are minor; however, the high trace density of today’s multilayer printed circuit boards and the large number of via holes with a diameter of 0.4 mm or less make this a serious problem. One solution is the ZM process, in which zinc and sulphuric acid are used to minimise red ring formation. The following reaction takes place:
Zn + H₂SO₄ → ZnSO₄ + 2H;
CuO (red ring) + 2H → Cu + H₂O
As zinc has a lower electrochemical potential than copper, it acts as a ‘sacrificial anode’ and dissolves before the copper oxide does, thereby protecting the latter from reduction. → Black oxide treatment
Foaming fluxer
A common device for evenly coating the underside of a printed circuit board with flux prior to wave soldering. In this process, compressed air is fed through a foaming tube into a tank to foam up the flux contained therein, which is then distributed across the underside of the printed circuit board. However, with this method, it is difficult to control the thickness of the flux layer, and the result is usually a relatively thick coating. Furthermore, the foamed flux evaporates more readily, leading to high overall consumption. The coated surface is also sticky and therefore prone to contamination. Depending on the operating temperature, the composition of the solvent and its concentration must therefore be adjusted separately. Flux that has foamed up too much can also pass through to the top side of the printed circuit board and contaminate the components. If flux penetrates, for example, into a switch element, this can lead to contact faults later on.
Black oxide treatment
Shiny copper surfaces on the inner layers of multilayer printed circuit boards are easily wetted and clean, but do not adhere well to synthetic resin and must therefore be roughened. This can be achieved through a chemical process known as black oxide treatment. To do this, the printed circuit board is immersed for 2 minutes at 95 °C in an oxidising agent consisting of 31 g of sodium chlorite, 15 g of sodium hydroxide and 12 g of sodium phosphate per litre of water (pH 13.4). This method achieves a high peel strength of 1.8–2.1 kg/cm². However, the duration of resistance to red ring formation is reduced by 2 minutes. The name derives from the black colouration of the copper following the treatment. If the colour is more brownish, the process is referred to as a brown oxide treatment. → Brown oxide treatment, → Red ring formation
Threshold limit value
The minimum physical quantity that must be added to a system to trigger a specific reaction or phenomenon. Also simply referred to as a limit value or TLV. For example, the limit value for the concentration of vapour from a tubular solder with a flux core is 3 mg/m³ of air. The decomposition products are measured on the basis of formaldehyde, but also include acetone, methyl alcohol, aliphatic aldehydes, carbon dioxide, carbon monoxide, methane, ethane, abietic acid, diterpene acid, etc.
Self-alignment effect
A phenomenon in which an SMC (surface-mounted chip) is aligned during reflow soldering by the surface tension of the molten solder, so that it is positioned exactly in the centre of the solder pad. This effect can compensate for slight displacements of the components during the placement process. → Surface tension.
Self-fluxing brazing
Brazing alloys that contain a reducing agent and thus act as a flux during the soldering process itself. In copper-phosphorus brazing alloys (5–7 % P, balance Cu), for example, the phosphorus acts as a deoxidiser. During brazing, it reduces the copper oxides and escapes into the atmosphere as gaseous phosphorus pentoxide (P₂O₅).
Selective oxidation (preferred oxidation)
Increasing the oxidisability of an alloy by adding oxygen-affine elements. If, for example, a copper-tin alloy containing 20 % tin is allowed to oxidise, as shown in Figure (a), a dense coating of ZnO forms on the surface of the oxide layer because the oxygen-affine tin diffuses towards the oxide layer and the interface with the air. This prevents further oxidation of the base material. Figure (b) shows the formation of a multilayer oxide layer with a high content of base metals in alloys of iron with Al, Si, Cr, etc., which makes the material as a whole more resistant to oxidation. This layer formation is utilised in stainless steel.
A Sn–Pb solder alloy with added bismuth forms a Bi₂O₃ layer, which, due to its dull colour, facilitates visual inspection. This, too, is attributable to the selective oxidation of bismuth. Similarly, when a silver-tin alloy is heated, a layer of zinc oxide forms, which counteracts the formation of silver sulphide on the surface. Consequently, no black discolouration occurs due to sulphuric acid gas. If solder alloys contain zinc, selective oxidation also takes place and the metal becomes coated with zinc oxide. However, as the ZnO coating is mechanically fragile, such an alloy is unsuitable for soldering.
Selective reaction
Refers to the phenomenon whereby, when several chemical reactions are possible, one in particular takes precedence. In the manufacture of solder paste, for example, selectively reacting substances are added to induce a stepwise reaction sequence. Note: this is not the same as selective oxidation.
Silver chromate test paper
Test paper specified by the IPC J-STD-004B industry standard (test method described in IPC-TM-650, Method 2.3.33). If it is placed in a rinsing solution used to extract solder residues, the presence of the halogens chlorine and bromine can be detected by the discolouration of the reddish-brown Ag₂CrO₄ test paper. The size of the discoloured area is proportional to the concentration of chlorine and bromine. The following chemical reaction takes place:
Ag₂CrO₄ + 2 Cl⁻ → 2 AgCl (white) ↓ + CrO₄²⁻ + 2 Br⁻ → 2 AgBr (yellow) + CrO₄²⁻
Silver brazing alloy (silver solder)
An Ag-Zn-Cu alloy, which is mainly used in brazing and has a relatively low melting point, high fluidity and high corrosion resistance. The possible compositions are shown in the table. The addition of P, Ni, Cd, Mn and Sn can lower the melting point and increase fluidity.
Chemical composition of silver brazing alloys (%)
Ag Cu Zn Other Melting point (°C) Application
10 52 38 790 for steel
15 80 P 5 640 Sil-Fos
20 45 30 Cd 5 yellow solder
20 45 35 780
33 38 32 740
33 50 17 Railway
40 14 6 Sn 40
40 36 24 720
45 17 18 Cd 20 625
45 30 25 680
50 33 17 Brass
50 15.5 16.5 Cd 18 630 Easy-flow
56 22 17 Sn 5 630 Ready-flow
60 20 15 Ni 5 for high loads
65 20 15 for nickel
70 20 10 for steel
72 28 780 for copper
80 13.5 6.5 for hard alloys
85 Mn 1 for high temperatures
Chemical composition of silver brazing alloys (%)
SMOBC
Abbreviation for Solder Mask Over Bare Copper. A process in which the solder mask is applied directly to the bare copper. This improves the solderability of the exposed connection pads. To achieve this, for example, the printed circuit board with the solder mask is tin-plated using hot air and then soldered.
Solder balling test
This test, which is included in the standard specifications for Phillips solder paste (UN-L), is designed to verify the reflow suitability of a solder paste on a non-wettable substrate. To do this, an adhesive film 0.1 ± 0.001 mm thick with an opening of 5.5 ± 0.1 mm is adhered to an aluminium oxide plate that solder does not wet (thickness 0.6–0.8 mm, length 50 mm, width 25 mm) and a small amount of solder paste is applied to the opening. The adhesive film is then removed using a spatula, leaving a layer of solder paste approximately 0.07 mm thick and with a diameter of 5.5 ± 0.1 mm. The distance between individual holes of this type should be at least 10 mm. The plate is then heated above a solder bath with the coated side facing upwards. The result is to be assessed in accordance with the table below. The test is carried out on samples that have been stored under normal atmospheric conditions for 0, 24 and 72 hours, respectively, after the solder paste has been applied. The test is also described in IPC TM650.
Solidus line
The temperature, plotted as a function of an alloy’s composition, at which the cooling melt of that alloy solidifies completely is called the solidus line, analogous to the liquidus line. Between these two lines, the metals exist as a mixture in both liquid and solid phases.
A’ A’’ E – Primary crystal A (solid phase) and eutectic (liquid phase)
B’ B’’ E – Primary crystal B (solid phase) and eutectic (liquid phase)
In a eutectic alloy, therefore, the solidification process is complete upon reaching the solidus line, i.e. the eutectic temperature. The diagram refers to a eutectic system consisting of A and B, whereby the hatched areas – that is, the triangles A‘ A‘‘ E and B‘ B‘‘ E – correspond to the region of phase mixtures enclosed by the liquidus and solidus lines.
Solvus line (solvus)
Also known as the solubility line. In an alloy comprising several substances, solid phases begin to precipitate from the solid solution at a certain temperature below the solidus line. The solvus line or surface indicates the composition of these phases, which are in equilibrium with one another, as a function of temperature and pressure within the phase diagram. In a binary system at constant pressure, this takes the form of a curve; in a ternary system, it is a surface. If the solvus and solidus lines do not intersect, there exists a temperature/pressure range in which the system forms a stable, continuous solid solution. Otherwise, only partial solid solutions are formed. In the solder alloy (Sn–Pb system), tin precipitates from the lead solution along the solvus line below the eutectic temperature.
Butt soldering
Refers to the process of soldering two metal sheets together at their edges. Such a joint cannot possess high tensile or flexural strength. In butt welding, which is a resistance welding process, an electric current is passed through the parts to be welded, and the weld zone is melted and joined by the heat generated by electrical resistance. Spot welding and seam welding also operate on this principle.
Sub-grain
When a metal solidifies, spatially aligned groups of atoms form crystal grains. Subgrains are smaller sub-crystals within these grains. By deep etching a solder, it is possible to make tiny lines visible in the Sn and Pb crystals, as shown in the figure. These are the sub-grains, each of which has its own orientation. The boundaries of these units are referred to as sub-grain boundaries.
Sublimation
The transition of a substance from the solid to the gaseous state, and vice versa, without first becoming liquid. Among other substances, sulphur sublimates when heated. At room temperature and standard pressure, camphor, iodine and CO₂ (dry ice), for example, sublimate. As sublimation is an endothermic process, dry ice is also used to cool solder paste during storage and transport. This inhibits chemical reactions that would otherwise take place at room temperature.
Substrate
A board used in the manufacture of printed circuit boards, onto which transistors and other components are mounted. This usually involves coating a plastic board with a copper foil, from which the circuit pattern is then etched. Thin ceramic plates (primarily made of aluminium oxide, Al₂O₃), which are coated with a conductive paste, can also serve as a substrate for mounting electronic components (ceramic substrate). In the latter case, substrates are frequently made from ALN (aluminium nitride). As the conventional substrates mentioned above have low thermal conductivity, it is also common practice to insulate metallic aluminium by means of anodic oxidation (Al₂O₃) and to mount the electronic components on top of this. These so-called metallic substrates prevent the assembly from overheating.
Superconductor (super conductor, supra conductor)
Normally, the electrical resistance of metals increases as the temperature rises. Conversely, it decreases as the temperature falls. As the temperature approaches absolute zero, i.e. –273 °C, the resistance of some materials also approaches zero. The temperature beyond which the resistance suddenly decreases sharply is known as the critical temperature Tc.
The figure shows the critical temperatures of various metals. Plotted on the Y-axis is the ratio of W (the resistance of the metal at a given temperature) to Wo (the resistance at 0 °C).
When W/Wo equals 0, the state of absolute superconductivity is reached. Historically, intermetallic compounds such as Nb₃Sn and Nb₂Zr were first used in superconducting cables, as their Tc is 18 K (absolute temperature) and thus higher than that of pure metals. However, this requires liquid helium to cool the conductor to close to absolute zero. In 1986, a ceramic superconductor consisting of Y-Ba-Cu oxides was invented, which immediately attracted considerable attention. The invention was significant because, instead of expensive helium cooling, cheaper liquid nitrogen cooling (-210 °C) was sufficient. The ceramic superconductor does, however, have a number of disadvantages: its current density is low (i.e. it loses its superconductivity under high current), it is water-soluble and therefore sensitive to moisture, and there are limits to the strength of the magnetic field it can withstand. However, the foreseeable progress in thin-film production by vapour deposition suggests that such superconductors could soon be used in printed circuit boards. Research into suitable solders for superconducting printed circuit boards will then also become important. In the 21st century, superconductors could play an important role in projects such as electricity generation using superconducting magnetic coils, the construction of high-speed ships or maglev trains, or electricity storage. A maglev train, for example, in which the carriages hover above the track thanks to superconductivity, could cover the Berlin–Amsterdam or Berlin–Warsaw routes in two hours, or the Berlin–Budapest route in three hours.
Suspension
A liquid in which solid particles are dispersed. If the particles are colloids, the term ‘colloidal suspension’ (suspensoid) is used. Many industrial products, such as solder paste, paint or coatings, are suspensions. Their rheological properties, such as viscosity and fluidity, require special consideration. In particular, characteristics such as rheopexy, thixotropy and dilatancy are of significance here. → Rheopexy, → Thixotropy
Sweating/Leakage (sweating)
If, during press soldering or brazing, pressure is applied to the joint from the outside once the solder or filler metal has melted, liquid solder may escape. By analogy with the human body, this is also referred to in English as ‘sweating’. One form of press-soldering involves tin-plating the surfaces to be joined before soldering, so that a good bond forms during the pressing process. This is known as ‘sweat-joining’.
TAB
Abbreviation for Tape Automated Bonding. At present, plastic film (tape) with a diameter of 35 mm is predominantly used, although widths of 16 and 8 mm have also become common recently. In this process, the film is first coated with copper and etched, after which the chip is placed on it and wired using a suitable soldering process. This assembly method is used in particular in the mass production of watches and other devices with very small circuits.
Duty ratio
The finer the pitch of a printed circuit board, the more likely electromigration is to occur. A major factor here is the duty ratio of the pulse currents, which is defined as the ratio of the maximum to the average pulse power. If the conditions for migration are, for example, 65 °C, 95 % relative humidity, voltage (70 Hz, single electrode) 50 V, and a trace spacing of 0.1 mm, then migration occurs with a probability of over 30 % at a duty ratio of 0.5 or higher. (Tsukui, Kushida, Nagatanigawa: Denshijouhou Gakkai Gakujutsu Kenkyu Hokoku [Research Reports of the Society for Electronics and Information Technology], Vol. 90, No. 9, 1990, p. 29.) → Electromigration
Dew point
The surface temperature at which dew drops begin to form on a body cooling in air. If components cool overnight in a workshop with high humidity, water may condense on their surface and hinder soldering, or lead to the formation of blowholes. The parts to be soldered must therefore first be dehumidified by heating. The air in contact with the object is saturated with water vapour, and the partial pressure of the water vapour corresponds to the saturation vapour pressure at the dew point. The relative humidity can therefore be determined using a dew point hygrometer, which, for example, gradually cools a metal mirror and measures the temperature at which it becomes fogged up.
TCE
Abbreviation for thermal coefficient of expansion. When manufacturing multilayer printed circuit boards, it is essential to take into account the coefficients of thermal expansion of the respective materials. This coefficient is also a common cause of faulty solder joints. Matching the coefficients of thermal expansion is therefore an important consideration when designing solder joints.
Surfactant (surface-active agent)
The term ‘surface active agent’ is abbreviated to ‘surfactant’ in English. Surfactants ensure high surface activity at the surface of the solvent and are both hydrophilic and lipophilic. Thanks to their balanced solubility, they promote adsorption at phase boundaries and significantly reduce the free energy at the interface. They are therefore used not only as detergents but also in many other areas due to their emulsifying, foaming, dispersing and solubilising effects. They are mostly synthetic products, although natural surfactants, such as gelatine, also exist.
Thermal stress (internal thermal stress)
The cooling of a body from a given temperature never takes place uniformly throughout the body, unless the cooling process is extremely slow. Normally, some areas cool down faster than others and consequently contract more than the parts that are still warmer. This variation in the degree of contraction leads to internal stresses within the cooling body. Solder joints and castings therefore often contain internal thermal stresses that have arisen during cooling. Thorough annealing prior to use is therefore essential, particularly for large castings, as otherwise deformation may occur.
Thermite process
A technique for reducing or welding metal oxides by utilising the large amounts of heat released during the oxidation of aluminium and other easily oxidised metals. When aluminium is used as the reducing agent in this process, the term ‘aluminothermy’ is employed. In this process, the metal oxide is mixed with aluminium, manganese or an alloy of the two in powder form and ignited. The metal oxide oxidises the aluminium and manganese and is itself reduced, melting into a lump due to the heat of reaction. Chromium oxide Cr₂O₃, for example, is reduced by aluminium as follows:
Cr₂O₃ + 2 Al → 2 Cr + Al₂O₃ + 112 kcal
The welding and joining of metal using this method is known as thermite welding. For this purpose, powdered aluminium or magnesium, or an aluminium-magnesium alloy, is applied to the joint and ignited, so that the parts to be joined melt at the joint due to the heat of oxidation and bond together. Thermite welding was formerly used to join iron rails.
Thermal bar soldering / hot bar reflow soldering
First, the component is picked up automatically or semi-automatically and placed, together with a 0.008–0.03 mm thick layer of solder, onto a circuit pattern that has already been coated with flux. A profiled thermode (hot bar) then presses the lead wires down. If these do not yet touch the contact pad, the pressure is increased. The contact pressure is preset. Once the reflow soldering time has elapsed, the thermode releases and the component’s soldering cycle is complete. The thermode is interchangeable depending on the size of the component. Complex profiles can be created in line with the requirements of the manufacturing process to solder several components simultaneously. → Press soldering
Thermocouple pair (thermocouple)
If, as shown, two different metallic conductors, A and B, are connected to one another and different temperatures prevail at the contact points m and n, a potential difference arises within this circuit and a direct current flows. This phenomenon is known as the Seebeck effect. If point m is at room temperature and point n is exposed to a higher temperature, the temperature at point n can be calculated from the current measured in the circuit. Conversely, a temperature difference arises between points m and n when a current is applied to the circuit; this is known as the Peltier effect. The metal pair is referred to here as a thermocouple pair. Depending on the temperature to be measured, the pairs listed in the table below are used.
For temperature measurement during soldering, the Ni-Cu pairs (Constantan/copper or Constantan/iron) are sufficient; however, in view of the risk of corrosion at high temperatures, Alumel/Chromel is more commonly used.
This pair is also widely used for temperature measurements in SMT reflow ovens or when melting solder alloys.
Composition and operating temperature of thermocouple pairs (: denotes pair)
Measurement temperature (°C) 0–400 400–900 900–1400
Thermocouple pairs and their chemical composition Cu : Constantan
Fe: Constantan Alumel (Ni94; Al2; Si1; Fe0.5; Mn2.5) : Chromel (Ni89; Cr9.8; Fe1; Mn0.2) Pt : Pt-Rh(10)
Composition and operating temperature of thermocouple pairs (: denotes a pair)
Thixotropy
A property of solder paste made from solder powder and flux. The gel transforms into a liquid sol simply by mixing and kneading, but if left to stand in this state for a while, it loses its fluidity and reverts to a gel. This applies in particular to substances whose colloidal particles exhibit plastic anisotropy, have only weak bonds between the particles and readily form gels. Factors influencing this include the shape and size of the particles, their surface properties and the dispersing agent. In solder paste, under the influence of external forces, the internal cohesion of the gel decreases or is lost, causing it to become a sol and thereby acquire greater fluidity. When the external forces cease, the particle bonds regenerate and the fluidity decreases once more. If the fluidity returns to its initial state more slowly than the bonds are broken, the paste exhibits significant hysteresis. This ratio is used to quantify thixotropy. In some cases, however, only the time taken to return to the gel state (setting time) is used. Accordingly, solder paste should be used as quickly as possible after production.
Triclene
Trade name for trichloroethene (CHC=CCl₂), produced from acetylene and chlorine. It was formerly commonly used to degrease electronic components prior to soldering, but is now banned as a hazardous substance due to its chlorine content. It is a colourless, non-flammable liquid with a melting point of –70 °C, a boiling point of 87 °C and a specific gravity of 1.459. Trichloroethene is not soluble in water, but is miscible with common organic solvents. It has a high solvent power and a cleaning power many times greater than that of petrol. When used in vapour form, it is also known as Triclene D. The cleaning effluent must be treated with activated carbon before disposal.
Excess solder
If there is excess solder at the solder joint, it can rise up between the lead wires, particularly in the case of components with a small pin pitch (SOPs). To remove the excess solder, use desoldering braid or, in the case of wave soldering, an air knife. → Air knife, → Desoldering braid
Clinching
Bending the connection ends of components on the reverse side of the printed circuit board during through-hole assembly to prevent them from detaching. If the bending angle is too small, the components will easily come loose from the board; however, if the angle is too large, the lead may snap off. An angle of approximately 5–15° relative to the board surface is therefore considered appropriate.
V-cut
When soldering with cored solder, the temperature of the solder causes the flux inside the solder to boil, causing it to splash out as soon as the surrounding solder shell melts away, resulting in the formation of solder bumps. To prevent this, a V-shaped incision is made along the axis of the cored solder, allowing the flux to evaporate when the cored solder melts, without causing explosive splashes of solder. However, cored solder with an incision cannot be stored for long because the flux oxidises. Therefore, the incision is usually made just before soldering. See also Splashing.
Magnification ratio, distortion ratio
To examine the microscopic structure at the tip of a soft solder such as Sn-Pb, it is advisable to coat this tip with a layer of copper beforehand. As the layer is very thin, the structure observed under the microscope appears magnified when the ground specimen is positioned at a specific angle. The magnification factor referred to here relates to this effect. The figure shows a cross-section of a base material sample fixed at an angle. The angled cut normally achieves a tenfold magnification, with an angle of 5° 44′ 21″ (nominally 6°) frequently being used, as shown in the image. Sometimes the specimen is mounted in a distorted form, in which case the term ‘distortion ratio’ is used.
Fusing (solder fusing)
A process step in the manufacture of through-hole printed circuit boards, in which, following the formation of the conductor pattern using a solder layer (metallisation) as an etching mask, the solder layer is melted by heating and fused into a continuous alloy. To melt the solder layer, either infrared radiation or an oil or glycerine bath heated to 200–220 °C is used, into which the through-hole printed circuit board is immersed. The former process is known as infrared fusing, whilst the latter is known as oil fusing. This treatment serves to prevent short circuits between conductor tracks caused by overhanging solder, to ensure the solder layer is homogeneous, and to improve solder penetration in the through-holes. → Red ring formation, → PTH
Tinning
Solder plating. This process of applying a layer of solder to the solder joints is often carried out during the manufacture of printed circuit boards prior to the actual soldering. The term ‘pattern plating’ (tin plating of the circuit pattern) is also used to describe this process. The alloy used for this purpose is usually pure tin.
White residue
White flux residues found scattered across printed circuit boards. On closer inspection, these are often more yellow or grey in colour and are, in such cases, also referred to as grey or yellow residues.
Unlike rosin-based flux in general, flux containing organic acids is difficult to remove, particularly when residues remain after soldering at temperatures of 250 °C or higher. Even after cleaning with a solvent, water-insoluble white residues may remain on the printed circuit board under certain circumstances. Whilst these have virtually no effect on the insulation resistance at room temperature, they can lead to corrosion at higher temperatures. In this case, it is necessary to change the composition of the flux, carry out a particularly thorough cleaning, or use a specialised cleaning agent.
Water White, WW
‘Water white’ means ‘crystal-clear’ and refers to the colour of the rosin. According to the ASTM standard, WW is the purest form of rosin; in the US standard, however, this is identical to type ‘R’. As the industrial designation ‘non-activated rosin’ suggests, it has very low chemical reactivity and is therefore usually combined with a suitable activator for use as a soldering flux.
Value analysis (value engineering, VE)
Value analysis (VA) is based on the idea that the value of a good varies depending on time, circumstances and place (Time, Occasion, Place = TOP). For example, even a match has great value if you are on a mountain summit and have no other way of lighting a fire to keep warm. Soldering involves many steps, including pre-treatment. H.H. Manko therefore attaches great importance to the coordination of work processes and considers optimisation through VA to be the most efficient approach to organising them.
Whisker
A ‘whisker’ refers to a crystal in which the atoms form a homogeneous crystal lattice without any defects. This phenomenon first came to public attention following a disruption to the New York telephone network caused by a short circuit in a telephone line. Under the influence of electrical resistance heat (I²R), a high-purity, needle-shaped tin crystal had grown within the tin sheath of the copper cable, piercing the outer wall of the cable and destroying its insulation.
Due to their needle-like growth, such crystals are called whiskers. As this anecdote illustrates, such a whisker is strong enough to pierce a cable. In theory, it would be possible to use such crystals to manufacture, for example, suspension cables for bridges that would be much finer than conventional suspension systems. However, the production of whiskers has so far been limited to the crystallisation of dissolved substances from saturated aqueous solutions and other experimental methods, and is not expected to be ready for mass production in the foreseeable future. The commercial term ‘gypsum whisker’, which is sometimes encountered, is misleading and is intended merely to suggest a particularly strong fibre.
Resistance in solution (solution resistance)
A method for determining the insulating properties of a soldering flux, as set out in the JIS-Z 3197-1986 standard. The aim here is to determine the electrical resistance of tubular solders, solder paste, liquid and solid fluxes, and fluxes containing rosin in aqueous solution.
The samples are prepared in accordance with the following table:
Type of flux Sample preparation
Tube solder with flux core Extraction using a 35 % isopropyl alcohol solution
Solder paste Liquid flux
Liquid flux Finished product
Solid flux Finished product
Rosin-based flux Finished product
The samples are prepared as shown in the following table:
A sufficient quantity of the above samples is poured into a beaker containing 50 ml of demineralised water, which is then covered with a watch glass, heated and brought to the boil within approximately 5 minutes. Allow it to boil for a further minute or so, then leave it to cool at room temperature for approximately 10 seconds. It is then cooled in a water bath at approximately 20 °C and is then ready for testing. The resistance in the test liquid is then measured immediately using a conductometer.
Remelting press-soldering
In this process, an alloy layer is first formed at the interface between the solder and the base material. This joint is then reheated and, as soon as the solder melts, compressed. The solder, with its low melting point and low strength, is forced out of the solder gap in its liquid state, and the alloyed layers bond directly with one another. Viewed under a microscope, this produces the following image:
Figure A shows the state after soldering two parts. A considerable amount of solder is present at the joint. Figure B was taken after pressing at the solder’s melting temperature. Most of the solder has been pressed out of the gap and the parts are joined together with almost no solder layer. As the diagram illustrates, pressing can be combined with rapid heating of the components by means of electrical resistance. This topic is discussed in the following research paper: Hattori, Funamoto, Shida (Hitachi Ltd.), ‘Properties of Joints in Resistance-Heated Press Soldering’, Proceedings of the Japan Welding Society, Vol. 7 (1989), No. 3, pp. 348–351.
Age-related softening
Immediately after soldering with a Sn-Pb alloy, the dendrites in the solder are supersaturated with tin. If the solder is left to stand at room temperature for a few days, the excess tin precipitates and the solder softens; this is also due to the reduction in internal mechanical stress. This is therefore referred to as age softening. Figure 1 shows a microscopic image of the solder that has just solidified. Figure 2 shows the precipitation of tin. The addition of antimony counteracts this age softening.
Centrifugal atomisation (centrifugal atomising process)
A method used primarily for the production of solder powder for solder paste, in which molten solder flows through tiny holes onto a rapidly rotating disc under vacuum or in an inert gas, so that the molten material is flung out by centrifugal force and solidifies into fine solder powder. There is hardly any oxidation during this process, and spherical solder particles can be produced. Consequently, this process has recently superseded gas atomisation – where it is more difficult to obtain round solder particles – and is frequently used in the production of solder powder for solder paste.
Tin pest
Tin occurs in the α-Sn and β-Sn forms. The latter transforms into α-Sn at –30 °C, whereby the metallic β-Sn swells like an ulcer and then disintegrates very easily. This is due to the fact that, at a certain temperature threshold (–30 °C), tin undergoes a phase transformation and its coefficient of thermal expansion changes abruptly. Furthermore, the coefficient of expansion is isotropic in β-Sn, whilst it is anisotropic in α-Sn. However, adding small amounts of antimony, lead or bismuth to the tin prevents tin pest. For this reason, British and American solder standards previously stipulated the addition of antimony. However, even so-called pure tin contains minute quantities of lead, antimony and bismuth, which is why the mandatory addition of antimony is unnecessary. Consequently, this requirement has been removed from the standards. → Allotrope
Zone melting process
A refining process for the production of high-purity metal. This method was invented by the American W. G. Pfann for the refining of germanium. In the past, high-purity metals were produced by chemical means; however, this was expensive and therefore unsuitable for mass production. In contrast, the zone melting process, as a physical refining method, is not only cost-effective but also enables the refining of intermetallic and other compounds in addition to metals.
The principle is based on the observation that, when producing metal ingots from a melt, impurities always accumulate at the point cast last. In zone melting, therefore, a single- or double-turn heating coil is placed around the metal in the furnace and slowly moved along it. Of course, the metal can also be moved through the coil instead. In the case of horizontal movement, a ceramic boat is required for this purpose; however, this can itself be a source of impurities. To avoid this, a bare metal rod is positioned vertically and gradually lowered. This vertical process is used to refine silicon semiconductors, with the silicon being heated by a high-frequency induction coil. By repeating the zone melting process several times, the purity of the metal can be continuously increased.