This test, which is included in the standard specifications for Phillips solder paste (UN-L), is designed to verify the reflow suitability of a solder paste on a non-wettable substrate. To do this, an adhesive film 0.1 ± 0.001 mm thick with an opening of 5.5 ± 0.1 mm is adhered to an aluminium oxide plate that solder does not wet (thickness 0.6–0.8 mm, length 50 mm, width 25 mm) and a small amount of solder paste is applied to the opening. The adhesive film is then removed using a spatula, leaving a layer of solder paste approximately 0.07 mm thick and with a diameter of 5.5 ± 0.1 mm. The distance between individual holes of this type should be at least 10 mm. The plate is then heated above a solder bath with the coated side facing upwards. The result is to be assessed in accordance with the table below. The test is carried out on samples that have been stored under normal atmospheric conditions for 0, 24 and 72 hours, respectively, after the solder paste has been applied. The test is also described in IPC TM650.