Black oxide treatment
Shiny copper surfaces on the inner layers of multilayer printed circuit boards are easily wetted and clean, but do not adhere well to synthetic resin and must therefore be roughened. This can be achieved through a chemical process known as black oxide treatment. To do this, the printed circuit board is immersed for 2 minutes at 95 °C in an oxidising agent consisting of 31 g of sodium chlorite, 15 g of sodium hydroxide and 12 g of sodium phosphate per litre of water (pH 13.4). This method achieves a high peel strength of 1.8–2.1 kg/cm². However, the duration of resistance to red ring formation is reduced by 2 minutes. The name derives from the black colouration of the copper following the treatment. If the colour is more brownish, the process is referred to as a brown oxide treatment. → Brown oxide treatment, → Red ring formation